MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Ascend Performance Materials Vydyne® 47 NT Impact Modified Nylon 66
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, Impact Grade

Material Notes: Vydyne 47 NT is a general-purpose, medium impact-modified PA66 resin. 47 NT is recognized for all the processing and property advantages inherent to PA66 with the addition of improved impact strength. This resin offers a well balanced combination of engineering properties characterized by high melt point, good surface lubricity, abrasion resistance and resistance to many chemicals, machine and motor oils, solvents and gasoline. 47 NT is designed to meet the critical low-temperature impact requirements called out in many automotive specifications.

Information provided by Ascend Performance Materials.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.10 g/cc0.0397 lb/in³DAM; ISO 1183
Water Absorption 1.2 %
@Time 86400 sec
1.2 %
@Time 24.0 hour
DAM; ISO 62
Moisture Absorption at Equilibrium 2.3 %2.3 %DAM to 50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.018 cm/cm
@Thickness 2.00 mm
0.018 in/in
@Thickness 0.0787 in
DAM; ISO 294-4
Linear Mold Shrinkage, Transverse 0.016 cm/cm
@Thickness 2.00 mm
0.016 in/in
@Thickness 0.0787 in
DAM; ISO 294-4
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 40.0 MPa5800 psi50% RH; ISO 527-2
 52.0 MPa7540 psiDAM; ISO 527-2
Tensile Strength, Yield 45.0 MPa6530 psi50% RH; ISO 527-2
 60.0 MPa8700 psiDAM; ISO 527-2
Elongation at Break 22 %22 %DAM; ISO 527-2
 60 %60 %50% RH; ISO 527-2
Tensile Modulus 1.70 GPa247 ksi50% RH; ISO 527-2
 2.80 GPa406 ksiDAM; ISO 527-2
Flexural Strength 24.0 MPa3480 psi50% RH; ISO 178
 70.0 MPa10200 psiDAM; ISO 178
Flexural Modulus 0.800 GPa116 ksi50% RH; ISO 178
 2.30 GPa334 ksiDAM; ISO 178
Izod Impact, Notched (ISO)  12.0 kJ/m²
@Temperature -40.0 °C
5.71 ft-lb/in²
@Temperature -40.0 °F
DAM; ISO 180/1A
 16.0 kJ/m²
@Temperature -30.0 °C
7.61 ft-lb/in²
@Temperature -22.0 °F
DAM; ISO 180/1A
 18.0 kJ/m²
@Temperature -40.0 °C
8.57 ft-lb/in²
@Temperature -40.0 °F
50% RH; ISO 180/1A
 18.0 kJ/m²
@Temperature 23.0 °C
8.57 ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 180/1A
 24.0 kJ/m²
@Temperature -30.0 °C
11.4 ft-lb/in²
@Temperature -22.0 °F
50% RH; ISO 180/1A
 44.0 kJ/m²
@Temperature 23.0 °C
20.9 ft-lb/in²
@Temperature 73.4 °F
50% RH; ISO 180/1A
Charpy Impact Unnotched  NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
50% RH; ISO 179/1eU
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
DAM; ISO 179/1eU
 NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
50% RH; ISO 179/1eU
 NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
DAM; ISO 179/1eU
Charpy Impact, Notched  1.10 J/cm²
@Temperature -40.0 °C
5.23 ft-lb/in²
@Temperature -40.0 °F
DAM; ISO 179/1eA
 1.70 J/cm²
@Temperature -30.0 °C
8.09 ft-lb/in²
@Temperature -22.0 °F
DAM; ISO 179/1eA
 1.80 J/cm²
@Temperature -40.0 °C
8.57 ft-lb/in²
@Temperature -40.0 °F
50% RH; ISO 179/1eA
 1.90 J/cm²
@Temperature 23.0 °C
9.04 ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 179/1eA
 2.40 J/cm²
@Temperature -30.0 °C
11.4 ft-lb/in²
@Temperature -22.0 °F
50% RH; ISO 179/1eA
 6.20 J/cm²
@Temperature 23.0 °C
29.5 ft-lb/in²
@Temperature 73.4 °F
50% RH; ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+12 ohm-cm
@Thickness 1.00 mm
1.00e+12 ohm-cm
@Thickness 0.0394 in
DAM; IEC 60093
Dielectric Strength 24.0 kV/mm
@Thickness 1.00 mm
610 kV/in
@Thickness 0.0394 in
DAM; IEC 60243
Arc Resistance 120 - 180 sec
@Thickness 3.00 mm
120 - 180 sec
@Thickness 0.118 in
PLC 5; ASTM D 495
Comparative Tracking Index 600 V
@Thickness 3.00 mm
600 V
@Thickness 0.118 in
IEC 60112
Hot Wire Ignition, HWI 7.0 - 15 sec7.0 - 15 secPLC 4; UL 746
 7.0 - 15 sec7.0 - 15 secPLC 4; UL 746
 30 - 60 sec30 - 60 secPLC 2; UL 746
High Amp Arc Ignition, HAI >= 120 arcs>= 120 arcsPLC 0; UL 746
 >= 120 arcs>= 120 arcsPLC 0; UL 746
 >= 120 arcs>= 120 arcsPLC 0; UL 746
High Voltage Arc-Tracking Rate, HVTR 10.0 - 25.4 mm/min0.394 - 1.00 in/minPLC 1; UL 746
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 111 µm/m-°C
@Thickness 2.00 mm,
Temperature 35.0 - 55.0 °C
61.7 µin/in-°F
@Thickness 0.0787 in,
Temperature 95.0 - 131 °F
DAM; ISO 11359-2
CTE, linear, Transverse to Flow 136 µm/m-°C
@Thickness 2.00 mm,
Temperature 23.0 - 55.0 °C
75.6 µin/in-°F
@Thickness 0.0787 in,
Temperature 73.4 - 131 °F
DAM; ISO 11359-2
Melting Point 260 °C500 °FDAM; ISO 11357-3
Deflection Temperature at 0.46 MPa (66 psi) 185 °C365 °FUnannealed; DAM; ISO 75-2/B
Deflection Temperature at 1.8 MPa (264 psi) 63.0 °C145 °FUnannealed; DAM; ISO 75-2/A
UL RTI, Electrical  125 °C
@Thickness 0.750 mm
257 °F
@Thickness 0.0295 in
UL 746
 125 °C
@Thickness 1.50 mm
257 °F
@Thickness 0.0591 in
UL 746
 125 °C
@Thickness 3.00 mm
257 °F
@Thickness 0.118 in
UL 746
UL RTI, Mechanical with Impact  75.0 °C
@Thickness 0.750 mm
167 °F
@Thickness 0.0295 in
UL 746
 75.0 °C
@Thickness 1.50 mm
167 °F
@Thickness 0.0591 in
UL 746
 75.0 °C
@Thickness 3.00 mm
167 °F
@Thickness 0.118 in
UL 746
UL RTI, Mechanical without Impact  85.0 °C
@Thickness 0.750 mm
185 °F
@Thickness 0.0295 in
UL 746
 85.0 °C
@Thickness 1.50 mm
185 °F
@Thickness 0.0591 in
UL 746
 85.0 °C
@Thickness 3.00 mm
185 °F
@Thickness 0.118 in
UL 746
Flammability, UL94  HB
@Thickness 0.750 mm
HB
@Thickness 0.0295 in
 HB
@Thickness 1.50 mm
HB
@Thickness 0.0591 in
 HB
@Thickness 3.00 mm
HB
@Thickness 0.118 in
Glow Wire Ignition Temperature  750 °C
@Thickness 3.00 mm
1380 °F
@Thickness 0.118 in
IEC 60695-2-13
 775 °C
@Thickness 0.750 mm
1430 °F
@Thickness 0.0295 in
IEC 60695-2-13
 800 °C
@Thickness 1.50 mm
1470 °F
@Thickness 0.0591 in
IEC 60695-2-13
Glow Wire Flammability Index  725 °C
@Thickness 3.00 mm
1340 °F
@Thickness 0.118 in
IEC 60695-2-12
 750 °C
@Thickness 0.750 mm
1380 °F
@Thickness 0.0295 in
IEC 60695-2-12
 775 °C
@Thickness 1.50 mm
1430 °F
@Thickness 0.0591 in
IEC 60695-2-12
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 280 - 310 °C536 - 590 °FInjection
Middle Barrel Temperature 280 - 310 °C536 - 590 °FInjection
Front Barrel Temperature 280 - 310 °C536 - 590 °FInjection
Nozzle Temperature 280 - 310 °C536 - 590 °FInjection
Melt Temperature 285 - 305 °C545 - 581 °FInjection
Mold Temperature 65.0 - 95.0 °C149 - 203 °FInjection
Drying Temperature 80.0 °C176 °FInjection
Dry Time 4.00 hour4.00 hourInjection
 
Descriptive Properties
Agency RatingsASTM, D4066 PA0151
 ASTM, D6779 PA0151
AppearanceNatural Color
FeaturesAbrasion Resistance
 Chemical Resistant
 Gasoline Resistant
 General Purpose
 Good Processability
 Good Toughness
 High Impact Resistance
 Impact Modified
 Low Temperature Impact Resistance
 Low Temperature Toughness
 Oil Resistant
 Solvent Resistant
FormsPellets
Processing MethodInjection Molding
RegionNorth America, Europe, Asia Pacific
UL File NumberE70062

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Ascend Performance Materials Vydyne® 41 NT Impact Modified Nylon 66
Akro-Plastic Akromid® B3 S3 natural (3669) PA6-I, DAM
Borealis Daplen™ EE255AE Polypropylene TPO Compound
Borealis Daplen™ EE260AE Scratch Resistant Polypropylene Compound
Akro-Plastic Akromid® A3 S1 natural (2310) PA 6.6 Conditioned, Impact Modified

PASCE9705 / 220808

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.