MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

Bada BADAFORM® C110 GF25 natural POM, 25% Glass Fiber Reinforced
Categories: Polymer; Thermoplastic; Acetal (Polyoxymethylene, POM); Acetal Copolymer, 30% Glass Fiber Reinforced

Material Notes: 25% glass fiber reinforced acetal copolymer, injection molding grades

Information provided by Bada

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.59 g/cc0.0574 lb/in³ISO 1183
Moisture Absorption 0.170 %0.170 %50% r.h.; ISO 62
Water Absorption at Saturation 0.80 %0.80 %ISO 62
Melt Flow 4.0 g/10 min
@Load 2.16 kg,
Temperature 190 °C
4.0 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Ball Indentation Hardness 220 MPa
@Load 36.5 kg
31900 psi
@Load 80.5 lb
ISO 2039-1
Tensile Strength at Break 120 MPa17400 psi5 mm/min; ISO 527-1/2
Elongation at Break 2.0 %2.0 %5 mm/min; ISO 527-1/2
Tensile Modulus 9.30 GPa1350 ksi1 mm/min; ISO 527-1/2
Flexural Strength 160 MPa23200 psiISO 178
Izod Impact, Notched (ISO) 5.00 kJ/m²
@Temperature 23.0 °C
2.38 ft-lb/in²
@Temperature 73.4 °F
ISO 180/1A
Charpy Impact Unnotched 3.00 J/cm²
@Temperature 23.0 °C
14.3 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eU
Charpy Impact, Notched 0.450 J/cm²
@Temperature 23.0 °C
2.14 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+14 ohm-cm1.00e+14 ohm-cmIEC-62631-3-1
Surface Resistance 1.00e+13 ohm1.00e+13 ohmIEC-62631-3-1
Dielectric Constant 4.5
@Frequency 1e+6 Hz
4.5
@Frequency 1e+6 Hz
IEC-62631-2-1
Dielectric Strength 25.0 kV/mm635 kV/inIEC-60243-1
Dissipation Factor 0.0095
@Frequency 1e+6 Hz
0.0095
@Frequency 1e+6 Hz
IEC-62631-2-1
Comparative Tracking Index 600 V600 VIEC-60112
 
Thermal PropertiesMetricEnglishComments
Melting Point 167 °C333 °F10 K/min; ISO 3146
Maximum Service Temperature, Air 100 °C212 °Fsome hours; EC-60216
Deflection Temperature at 1.8 MPa (264 psi) 160 °C320 °FISO 75-1/2
Vicat Softening Point 160 °C320 °FVST B50; ISO 306
Flammability, UL94 HB
@Thickness 1.60 mm
HB
@Thickness 0.0630 in
 
Processing PropertiesMetricEnglishComments
Melt Temperature 190 - 220 °C374 - 428 °F
Mold Temperature 70.0 - 100 °C158 - 212 °F
Drying Temperature 100 °C212 °F
Dry Time 1.00 - 3.00 hour1.00 - 3.00 hour
Moisture Content <= 0.20 %<= 0.20 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PBADA407 / 287240

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.