MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Chemours Viton® GBLT-600S with 10414 Fluoroelastomer Compound
Categories: Polymer; Thermoset; Fluoropolymer, TS; Thermoset Fluoroelastomer; Rubber or Thermoset Elastomer (TSE)

Material Notes:
  • GBLT-600S is an alternative to GLT and GFLT for fuel seals and fuel injector O-rings
  • Good fuel, methanol, and fluids resistance, improved vs. GLT
  • Low temperature Tg, TR-10, and sealing improved vs. Viton® GFLT
  • Heat resistance comparable to Viton® GLT-600S and GFLT-600S Good mold release / mold fouling properties
  • Good physical properties with high elongation, both original and aged
  • Good water and steam resistance / low volume swell in water
  • Excellent compression set resistance with either low or no postcure F169

Chemours was formed from former DuPont performance chemicals businesses, including the Viton product line, in 2015.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 68No Postcure; ASTM D1414
 714 hours Postcure; ASTM D1414
 718 hours Postcure; ASTM D1414
Tensile Strength at Break 8.50 MPaNo Postcure
 11.5 MPa4 hours Postcure
 12.6 MPa8 hours Postcure
Tensile Stress at Strain 1.00 MPa
@Strain 10 %
No Postcure; ASTM D412
 1.10 MPa
@Strain 10 %
4 hours Postcured; ASTM D412
 1.20 MPa
@Strain 10 %
8 hours Postcured; ASTM D412
Elongation at Break 248 %No Postcure; ASTM D412
 271 %8 hours Postcure; ASTM D412
 275 %4 hours Postcure; ASTM D412
100% Modulus 0.00530 GPa
@Strain 100 %
No Postcure; ASTM D412
 0.00690 GPa
@Strain 100 %
4 hours Postcured; ASTM D412
 0.00740 GPa
@Strain 100 %
8 hours Postcured; ASTM D412
Compression Set 14 %
@Temperature 200 °C,
Time 79200 sec
O-Rings, postcured; ASTM D395B
 20 %
@Temperature 200 °C,
Time 252000 sec
O-Rings, postcured; ASTM D395B
 23 %
@Temperature 200 °C,
Time 79200 sec
O-Rings, no postcure; ASTM D395B
 30 %
@Temperature 200 °C,
Time 252000 sec
O-Rings no postcure; ASTM D395B
 
Thermal PropertiesOriginal ValueComments
Minimum Service Temperature, Air -27.1 °CRetraction Temperature, Tr10; ASTM D1329
Glass Transition Temp, Tg -27.1 °C
 
Processing PropertiesOriginal ValueComments
Processing Temperature 177 °C
@Time 421 sec
Cure
 232 °C
@Time 14400 - 28800 sec
Postcure
 
Component Elements PropertiesOriginal ValueComments
Fluorine, F 66 %Uncompounded Viton
 
Descriptive Properties
Compound NumberA10-04
Silane TreatmentVinyl

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Chemours Viton® GBLT-600S with 10022 Fluoroelastomer Compound
Chemours Viton® GLT-200S Fluoroelastomer Compound
Chemours Viton® A-331C with Albaglos Fluoroelastomer Compound
Chemours Viton® A-331C with 60 MT Black Fluoroelastomer Compound
Chemours Viton® GBLT-600S with 10012 Fluoroelastomer Compound

PDVC9811 / 170452

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.