MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Rogers Corporation Poron® 4701-30-25 Urethane Foam, Very Soft
Categories: Polymer; Thermoset; Polyurethane, TS; Thermoset Polyurethane Foam, Unreinforced

Material Notes: Very soft, easily compressed for use where flexibility is a key requirement.  Standard available  thickness range from 0.021"

Features and Benefits of PORON Products:

  • Excellent compression set resistance which enables durable, long-term performance for gasketing, sealing, and cushioning.
  • Low-outgassing and non-fogging, containing no plasticizers or residual chemicals to contaminate the device. The material will not become brittle and crumble and is non-corrosive to metal.
  • Inherently flame retardant without the use of additives. Many of the materials meet flammability requirements of UL HBF and MVSS 302.
  • Engineered urethane formulations offering a wide modulus range - 2-90 psi @ 25% deflection – for more design versatility requirements.
  • Good chemical resistance
  • Easy to fabricate, die-cuts cleanly and works with a broad range of adhesives
  • Broad range of formulas and thicknesses from 0.012" to 0.500" (0.43mm to 12.7mm)

Applications:Communications

  • Automotive
  • Electronics
  • Other industrial equipment and devices

    Information provided by Rogers Corporation.

  • Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
     
    Physical PropertiesOriginal ValueComments
    Density 25.0 lb/ft³ASTM D3574-95 Test A
    Water Absorption 14 %Immersion; ASTM D570-95
    Moisture Absorption at Equilibrium 2.0 %High Humidity; AMS 3568-95
    Thickness 31.0 - 45.0 milRange of Thicknesses Available
    Outgassing - Total Mass Loss 0.60 %
    @Temperature 125 °C,
    Time 86400 sec
    WVR; at 7000 Pa; ASTM E595-93
     1.3 %
    @Temperature 125 °C,
    Time 86400 sec
    TML; at 7000 Pa; ASTM E595-93
    Collected Volatile Condensable Material 0.20 %
    @Temperature 125 °C,
    Time 86400 sec
    at 7000 Pa; ASTM E595-93
     
    Mechanical PropertiesOriginal ValueComments
    Hardness, Shore A 12ASTM D2240-97
    Hardness, Shore O 16ASTM D2240-97
    Tensile Strength >= 35.0 psiASTM D3574-75 Test E
     70.0 psiTypical; ASTM D3574-75 Test E
    Elongation at Break >= 100 %ASTM D3574-75 Test E
     150 %Typical; ASTM D3574-75 Test E
    Compressive Yield Strength 5.00 - 12.0 psi
    @Strain 25 %
    Range, 0.2"/min. strain rate
     9.00 psi
    @Strain 25 %
    Typical value, 0.2"/min. strain rate
    Tear Strength >= 0.700 kN/mASTM D264-91 Die C
     1.80 kN/mTypical; ASTM D264-91 Die C
    Compression Set 2.0 %
    @Temperature 23.0 °C
    ASTM D1667-90 Test D
     5.0 %
    @Temperature 121 °C
    autoclaved 5 hrs; ASTM D3574-95 J/Test D
     10 %
    @Temperature 70.0 °C
    ASTM D3574-95 Test D
     
    Electrical PropertiesOriginal ValueComments
    Volume Resistivity 3.00e+11 ohm-cmASTM D257-99
    Dielectric Constant 1.75
    @Time 86400 sec
    50% RH; ASTM D150
    Dielectric Strength 50.0 V/milASTM D149-97a
    Dissipation Factor 0.050ASTM D150-98
     
    Thermal PropertiesOriginal ValueComments
    CTE, linear 230 - 310 µm/m-°C
    Maximum Service Temperature, Air 90.0 °CConstant use; SAE J-2236
     121 °CIntermittent use; ASTM D746-98
    Brittleness Temperature -51.0 °CASTM D746-98
     
    Descriptive Properties
    Flammability TestpassMVSS 302; 0.062 in.

    Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

    Users viewing this material also viewed the following:
    Rogers Corporation Poron® 4790-79SP-15012 Urethane Shock Pad Foam
    Rogers Corporation Poron® 4701-30-15 Cellular Urethane Foam
    Rogers Corporation Poron® Shock Seal™ 4790-79-12 Urethane Foam, Industrial Grade
    Rogers Corporation Poron® ThinStik ShockSeal™ 79-09021 Self-Adhesive Urethane Foam
    Rogers Corporation Poron® 4701-15 Urethane Foam, Soft Seal

    PROGA912 / 138352

    Aluminum Castings

    Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

    The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.