MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Aardvark Polymers AARTEL® 2100UV Acetal Homopolymer Rotational Molding Resin
Categories: Polymer; Thermoplastic; Acetal (Polyoxymethylene, POM); Acetal Homopolymer, Unreinforced, Impact Grade

Material Notes:
  • Aartel 2100UV is a natural acetal homopolymer with UV stabilizers.
  • Aartel 2100UV is a medium viscosity resin with excellent flow characteristics.
  • Aartel 2100UV is available in natural white and may be painted, printed, or plated.
  • Aartel 2100UV may be compounded and dry colored.
  • Aartel 2100UV offers exceptional resistance to aggressive chemicals and fuels.
  • Aartel 2100UV has a fuel permeation rate of 1.2gr-mm/m2-day.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.42 g/cc
Water Absorption 0.50 %24 hour immersion
Moisture Absorption at Equilibrium 0.17 %50% RH
Water Absorption at Saturation 1.2 %
Linear Mold Shrinkage, Flow 0.020 cm/cm
@Thickness 2.00 mm
Linear Mold Shrinkage, Transverse 0.019 cm/cm
@Thickness 2.00 mm
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 92
Hardness, Rockwell R 120Test 1
 120Test 2
Tensile Strength, Ultimate 67.0 MPa5 mm/min (0.2 in/min)
Tensile Strength, Yield 67.0 MPa5 mm/min (0.2 in/min)
 70.0 MPa
Elongation at Break 30 %Nominal
 45 %5 mm/min (0.2 in/min)
Elongation at Yield 13 %5 mm/min (0.2 in/min)
 17 %
Tensile Modulus 3.10 GPa
 3.23 GPa5 mm/min (0.2 in/min)
Flexural Modulus 3.00 GPa
 3.05 GPa
Izod Impact, Unnotched 0.800 J/cm
Izod Impact, Notched (ISO) 8.00 kJ/m²
 8.00 kJ/m²
@Temperature -40.0 °C
Charpy Impact Unnotched 26.0 J/cm²
 26.0 J/cm²
@Temperature -30.0 °C
Charpy Impact, Notched 0.900 J/cm²
 0.800 J/cm²
@Temperature -30.0 °C
Impact 1870J/m; Unnotched
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+11 ohm-cmTest 1
 1.00e+14 ohm-cmTest 2
Surface Resistance 6.00e+14 ohm
Dielectric Constant 3.4
 3.5
@Frequency 100 Hz
 3.8
@Frequency 1e+6 Hz
Dissipation Factor 0.0060
@Frequency 1e+6 Hz
 0.018
@Frequency 100 Hz
Comparative Tracking Index 600 V
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 120 µm/m-°C
@Temperature 23.0 - 55.0 °C
 121 µm/m-°C
@Temperature 23.0 - 55.0 °C
CTE, linear, Transverse to Flow 120 µm/m-°C
@Temperature 23.0 - 55.0 °C
 120 µm/m-°C
@Temperature 23.0 - 55.0 °C
Melting Point 178 °C10°C/min
 178 °C
Deflection Temperature at 0.46 MPa (66 psi) 160 °C
 168 °CUnannealed
Deflection Temperature at 1.8 MPa (264 psi) 93.0 °C
 104 °CUnannealed
UL RTI, Electrical 50.0 °C
@Thickness 1.50 mm
 50.0 °C
@Thickness 3.00 mm
UL RTI, Mechanical with Impact 50.0 °C
@Thickness 1.50 mm
 50.0 °C
@Thickness 3.00 mm
UL RTI, Mechanical without Impact 50.0 °C
@Thickness 1.50 mm
 50.0 °C
@Thickness 3.00 mm
Flammability, UL94 HB
@Thickness 0.840 mm
Test 1
 HB
@Thickness 0.840 mm
Test 2
 HB
@Thickness 1.50 mm
Test 1
 HB
@Thickness 1.50 mm
Test 2
 HB
@Thickness 3.00 mm
Test 1
 HB
@Thickness 3.00 mm
Test 2
Oxygen Index 22 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aardvark Polymers AARTEL® 820UV Acetal Copolymer Rotational Molding Resin
LG Chemical LUCEL FW700S Modified POM, Friction Resistance, Abrasion Resistance
Ensinger Tecaform™ FG Blue Food Grade Acetal (POM)
Ensinger Delrin® 150 Homopolymer Acetal (POM)
Cheng Yu Plastic FV30G30 POM, 30% Glass Fiber

PGAPOLZ2 / 39218

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.