MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Alclad Aluminum 2024-T3
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 2000 Series Aluminum Alloy

Material Notes: General 2024 characteristics and uses (from Alcoa): Good machinability and surface finish capabilities. A high strength material of adequate workability. Has largely superseded 2017 for structural applications.

Uses: Aircraft fittings, gears and shafts, bolts, clock parts, computer parts, couplings, fuse parts, hydraulic valve bodies, missile parts, munitions, nuts, pistons, rectifier parts, worm gears, fastening devices, veterinary and orthopedic equipment, structures. Intrinsic corrosion resistance of 2024 is low for an aluminum alloy, so the clad version is used where needed.

Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes: Composition for AA 2024 (not Alclad 2024).
Composition information provided by the Aluminum Association and is not for design.

Key Words: UNS A82024; Alclad 2024-T3; Alclad 2024-T3; Al2024-T3
Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 2.78 g/ccFor AA2024 (Not Alclad)
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 65.0 ksiAA; Typical
 >= 400 MPa
@Thickness 0.203 - 0.229 mm
Flat sheet
 >= 405 MPa
@Thickness 0.254 - 1.57 mm
Flat sheet
 >= 420 MPa
@Thickness 1.60 - 3.25 mm
Flat sheet
 >= 425 MPa
@Thickness 3.28 - 6.32 mm
Flat sheet
Tensile Strength, Yield 45.0 ksiAA; Typical
 >= 270 MPa
@Thickness 0.203 - 0.229 mm
Flat sheet
 >= 270 MPa
@Thickness 0.254 - 1.57 mm
Flat sheet
 >= 275 MPa
@Thickness 1.60 - 3.25 mm
Flat sheet
 >= 275 MPa
@Thickness 3.28 - 6.32 mm
Flat sheet
Elongation at Break >= 10 %
@Thickness 0.203 - 0.229 mm
Flat sheet
 12 - 15 %
@Thickness 0.254 - 1.57 mm
Flat sheet
 >= 15 %
@Thickness 1.60 - 3.25 mm
Flat sheet
 >= 15 %
@Thickness 3.28 - 6.32 mm
Flat sheet
 18 %
@Thickness 1.59 mm
AA; Typical
Modulus of Elasticity 10600 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Shear Strength 40.0 ksiAA; Typical
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 775 °F
Solution Temperature 920 °F
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 90.7 - 94.7 %As remainder
Chromium, Cr <= 0.10 %
Copper, Cu 3.8 - 4.9 %
Iron, Fe <= 0.50 %
Magnesium, Mg 1.2 - 1.8 %
Manganese, Mn 0.30 - 0.90 %
Other, each <= 0.05 %
Other, total <= 0.15 %
Silicon, Si <= 0.50 %
Titanium, Ti <= 0.15 %
Zinc, Zn <= 0.25 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum 2024-T3
Alclad Aluminum 2024-O
Aluminum 6061-T6; 6061-T651
Alclad Aluminum 2024-T4, T351
Aluminum 7075-T6; 7075-T651

MA2024AT3 / 8859

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.