MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
AISI 1050 Steel, annealed at 790°C (1450°F)
Categories: Metal; Ferrous Metal; Carbon Steel; AISI 1000 Series Steel; Medium Carbon Steel

Material Notes: The composition listed applies only to structural shapes, plates, strip, and welded tubing. Semifinished products for forging, hot-rolled and cold-finished bars, wire rods, and seamless tubing have a carbon range of 0.48 - 0.55%.

Key Words: UNS G10500, EN43A, carbon steels
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.85 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 187
Hardness, Knoop 209Converted from Brinell
Hardness, Rockwell B 90Converted from Brinell
Hardness, Rockwell C 10Converted from Brinell hardness. Value below normal HRC range, for comparison purposes only.
Hardness, Vickers 196Converted from Brinell
Tensile Strength, Ultimate 635 MPa
Tensile Strength, Yield 365 MPa
Elongation at Break 24 %In 50 mm
Reduction of Area 40 %
Modulus of Elasticity 205 GPaTypical for steel
Bulk Modulus 160 GPaTypical for steel
Poissons Ratio 0.29Typical For Steel
Shear Modulus 80.0 GPaTypical for steel
Izod Impact 18.0 J
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000163 ohm-cm
@Temperature 0.000 °C
annealed specimen
 0.0000224 ohm-cm
@Temperature 100 °C
annealed specimen
 0.0000300 ohm-cm
@Temperature 200 °C
annealed specimen
 
Thermal PropertiesOriginal ValueComments
Specific Heat Capacity 0.486 J/g-°C
@Temperature >=100 °C
annealed
 0.519 J/g-°C
@Temperature 150 - 200 °C
 0.590 J/g-°C
@Temperature 350 - 400 °C
Thermal Conductivity 49.8 W/m-KTypical steel
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.47 - 0.55 %
Iron, Fe 98.46 - 98.92 %As remainder
Manganese, Mn 0.60 - 0.90 %
Phosphorus, P <= 0.040 %
Sulfur, S <= 0.050 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AISI 1050 Steel, normalized at 900°C (1650°F)
AISI 1050 Steel, cold drawn, 19-32 mm (0.75-1.25 in) round
AISI 1050 Steel, as rolled
AISI 1050 Steel, cold drawn, annealed, 19-32 mm (0.75-1.25 in) round
AISI 1050 Steel, normalized at 900°C (1650°F), air cooled, 13 mm (0.5 in.) round

M1050G / 7003

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.