MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Chemically Resistant adhesives

(Viewing data as-entered. Click here to return)
Menzolit Menzolit® HPC 1200 Unsaturated Polyester UP
Categories: Polymer; Thermoset; Polyester, TS; Thermoset Polyester Glass Filled BMC

Material Notes: HPC 1200 is a special SMC for high strength applications. The glass level has been selected to combine mouldability with high strength and stiffness properties in orientation direction. The reinforcement is composed of chopped, randomly distributed glass fibers and additional unchopped, continuous and lengthwise oriented glass fibers. This results in high strength and stiffness along with the unidirectional fibers. The flowability in orientation direction is reduced. This orientation influences flow during moulding and the anisotropic material properties have to be kept in mind during part design and part moulding. Typical applications are load bearing components, for instance bumpers and power train substructures.

Information Provided by Menzolit

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.80 g/ccISO 1183
Water Absorption <= 0.50 %ISO 62
Linear Mold Shrinkage -0.000300 cm/cmISO 2577
Linear Mold Shrinkage, Transverse 0.0025 cm/cmISO 2577
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 298 MPa
@Temperature 22.0 °C
25 mm flat samples, compression molded; ISO 527-4
Tensile Strength, Yield 298 MPa
@Temperature 22.0 °C
25 mm flat samples, compression molded; ISO 527-4
Elongation at Break 1.6 %ISO 527-4
Modulus of Elasticity 22.0 GPa25 mm flat samples, compression molded; ISO 527-4
Flexural Strength 655 MPa
@Temperature 22.0 °C
25 mm wide 100 mm long, flat samples; ISO 14125
Flexural Modulus 24.0 GPa
@Temperature 22.0 °C
25 mm wide 100 mm long, flat samples; ISO 14125
Compressive Yield Strength 350 MPaISO 14126
Poissons Ratio 0.30
Shear Modulus 8.46 GPaCalculated
Charpy Impact, Notched 25.7 J/cm²ISO 179
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+15 ohm-cmIEC 60093
Surface Resistance 1.00e+12 ohmIEC 60093
Dielectric Constant 4.0IEC 60250
Dielectric Strength 24.0 kV/mmIEC 60243-1
Dissipation Factor 0.010IEC 60250
Comparative Tracking Index 600 VIEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear 7.00 µm/m-°CISO 11359-2
Specific Heat Capacity 1.10 J/g-°C
Thermal Conductivity 0.700 W/m-K
Maximum Service Temperature, Air 170 °C
Deflection Temperature at 1.8 MPa (264 psi) >= 200 °CISO 75-2
Minimum Service Temperature, Air -40.0 °C
Glass Transition Temp, Tg 162 °CISO 11357-2
Flammability, UL94 HB
@Thickness 3.00 mm
Oxygen Index 22 %ISO 4589-2
Glow Wire Flammability Index 750 °CIEC 60695-2-12
 
Processing PropertiesOriginal ValueComments
Processing Temperature 135 - 150 °CCompression molding, matched metal die

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Menzolit Menzolit® HPC 1300 Unsaturated Polyester UP
Menzolit Menzolit® MMC 1600 Unsaturated Polyester UP
Menzolit Menzolit® SMC 0150 Unsaturated Polyester UP
Menzolit Menzolit® SMC 1100 Unsaturated Polyester UP
Menzolit Menzolit® SMC 1400 Unsaturated Polyester UP

PMENZ027 / 100761

Chemically Resistant adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.