MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

ALM Ultrasint® PA6 FR Nylon 6, Flame Retardant, Dry
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, Unreinforced, Flame Retardant

Material Notes: Ultrasint® PA6 FR is an advanced engineering polymer powder containing a flame-retardant (FR) additive.

Highlights:

  • Polyamide 6-based powder for Laster Sintering with flame retardant
Applications:
  • Switchboard parts and other electronic components
  • Media flow & storage parts (i.e. air ducts for buses/ aerospace)
  • Jigs & Fixtures for cables and pipes

Information provided by Advanced Laser Materials

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Bulk Density 0.550 g/cc0.0199 lb/in³DIN EN ISO 60
Density 1.30 g/cc0.0470 lb/in³Printed Part; DIN EN ISO 1181-1
Particle Size 65 - 75 µm65 - 75 µmD50
Melt Flow 13 g/10 min
@Load 2.16 kg,
Temperature 240 °C
13 g/10 min
@Load 4.76 lb,
Temperature 464 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 33.0 MPa4790 psiZ-Direction; ISO 527-2
 56.0 MPa8120 psiX-Direction; ISO 527-2
Elongation at Break 0.80 %0.80 %Z-Direction; ISO 527-2
 1.4 %1.4 %X-Direction; ISO 527-2
Tensile Modulus 4.50 GPa653 ksiZ-Direction; ISO 527-2
 4.75 GPa689 ksiX-Direction; ISO 527-2
Flexural Modulus 3.85 GPa558 ksiZ-Direction; DIN EN ISO 178
 4.40 GPa638 ksiX-Direction; DIN EN ISO 178
Izod Impact, Notched (ISO) 1.50 kJ/m²0.714 ft-lb/in²Z-Direction; ISO 180
 1.80 kJ/m²0.857 ft-lb/in²X-Direction; ISO 180
Izod Impact, Unnotched (ISO) 3.40 kJ/m²1.62 ft-lb/in²Z-Direction; ISO 180
 5.00 kJ/m²2.38 ft-lb/in²X-Direction; ISO 180
Charpy Impact Unnotched 0.250 J/cm²1.19 ft-lb/in²Z-Direction; ISO 179-1
 0.480 J/cm²2.28 ft-lb/in²X-Direction; ISO 179-1
Charpy Impact, Notched 0.100 J/cm²0.476 ft-lb/in²Z-Direction; ISO 179-1
 0.130 J/cm²0.619 ft-lb/in²X-Direction; ISO 179-1
 
Thermal PropertiesMetricEnglishComments
Melting Point 218 °C424 °FISO 11357
Crystallization Temperature 169 °C336 °FISO 11357
Deflection Temperature at 0.46 MPa (66 psi) 207 °C405 °FISO 75-2
Deflection Temperature at 1.8 MPa (264 psi) 113 °C235 °FISO 75-2
Vicat Softening Point  197 °C
@Load 5.10 kg
387 °F
@Load 11.2 lb
B; ISO 306
 214 °C
@Load 1.02 kg
417 °F
@Load 2.25 lb
A; ISO 306

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PALP9019 / 312354

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.