MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Envalior Durethan® DP BKV 240 H2.0 901510 Nylon 6 (PA6), 40% Glass Fiber Reinforced, Conditioned
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, 40% Glass Fiber Filled; Nylon 6, Impact Grade

Material Notes: 40% glass fiber, highest impact resistance

Former Lanxess product line is now with Envalior.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.41 g/cc0.0509 lb/in³ISO 1183
Linear Mold Shrinkage, Flow 0.0019 cm/cm0.0019 in/in150x105x3; ISO 2577
 0.0027 cm/cm0.0027 in/in60x60x2; ISO 2577
Linear Mold Shrinkage, Transverse 0.0074 cm/cm0.0074 in/in60x60x2; ISO 2577
 0.0078 cm/cm0.0078 in/in150x105x3; ISO 2577
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 90.0 MPa13100 psi5 mm/min; ISO 527-1,-2
Elongation at Break 7.5 %7.5 %5 mm/min; ISO 527-1,-2
Tensile Modulus 5.70 GPa827 ksi1 mm/min; ISO 527-1,-2
Flexural Strength 135 MPa19600 psi2 mm/min; ISO 178-A
Flexural Yield Strength 115 MPa
@Strain 3.5 %
16700 psi
@Strain 3.5 %
2 mm/min; ISO 178-A
Flexural Modulus 5.50 GPa798 ksi2 mm/min; ISO 178-A
Flexural Strain at Break 6.0 %6.0 %2 mm/min; ISO 178-A
Izod Impact, Notched (ISO)  15.0 kJ/m²
@Temperature -30.0 °C
7.14 ft-lb/in²
@Temperature -22.0 °F
ISO 180-1A
 35.0 kJ/m²
@Temperature 23.0 °C
16.7 ft-lb/in²
@Temperature 73.4 °F
ISO 180-1A
Izod Impact, Unnotched (ISO)  80.0 kJ/m²
@Temperature -30.0 °C
38.1 ft-lb/in²
@Temperature -22.0 °F
ISO 180-1U
 90.0 kJ/m²
@Temperature 23.0 °C
42.8 ft-lb/in²
@Temperature 73.4 °F
ISO 180-1U
Charpy Impact Unnotched 9.50 J/cm²
@Temperature 23.0 °C
45.2 ft-lb/in²
@Temperature 73.4 °F
ISO 180-1U
Charpy Impact, Notched 3.50 J/cm²
@Temperature 23.0 °C
16.7 ft-lb/in²
@Temperature 73.4 °F
ISO 180-1A
 
Thermal PropertiesMetricEnglishComments
Melting Point 210 °C410 °F10°C/min (Dry); ISO 11357-1,-3
 
Processing PropertiesMetricEnglishComments
Melt Temperature 290 °C554 °F
Mold Temperature 80.0 °C176 °F

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Wellman Wellamid® GS40-60 42L-NBK1 40% Glass Sphere Reinforced Nylon 6
Overview of materials for Nylon 6, 40% Glass Fiber Filled
Overview of materials for Nylon 6, 30% Glass Fiber Filled
Envalior Durethan® DP BKV 240 H2.0 901510 Nylon 6 (PA6), 40% Glass Fiber Reinforced, Dry
Envalior Durethan® BKV 240 H2.0 XCP 901510 Nylon 6 (PA6), 40% Glass Fiber Reinforced, Dry

PLANW9549 / 208355

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.