Physical Properties | Metric | English | Comments |
---|
Specific Gravity | 1.91 g/cc | 1.91 g/cc |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Shore A | 56 | 56 |
| 48 @Treatment Temp. 150 °C, Time 252000 sec | 48 @Treatment Temp. 302 °F, Time 70.0 hour |
| 52 @Treatment Temp. 125 °C, Time 252000 sec | 52 @Treatment Temp. 257 °F, Time 70.0 hour |
| 53 @Treatment Temp. 23.0 °C, Time 252000 sec | 53 @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 53 @Treatment Temp. 125 °C, Time 252000 sec | 53 @Treatment Temp. 257 °F, Time 70.0 hour |
| 54 @Treatment Temp. 100 °C, Time 252000 sec | 54 @Treatment Temp. 212 °F, Time 70.0 hour |
| 56 @Treatment Temp. 23.0 °C, Time 252000 sec | 56 @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 57 @Treatment Temp. 250 °C, Time 252000 sec | 57 @Treatment Temp. 482 °F, Time 70.0 hour |
| 57 @Treatment Temp. 275 °C, Time 252000 sec | 57 @Treatment Temp. 527 °F, Time 70.0 hour |
| 68 @Treatment Temp. 200 °C, Time 252000 sec | 68 @Treatment Temp. 392 °F, Time 70.0 hour |
Tensile Strength | 5.13 MPa | 744 psi |
| 2.426 MPa @Treatment Temp. 23.0 °C, Time 252000 sec | 351.9 psi @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 2.888 MPa @Treatment Temp. 200 °C, Time 252000 sec | 418.9 psi @Treatment Temp. 392 °F, Time 70.0 hour |
| 3.683 MPa @Treatment Temp. 150 °C, Time 252000 sec | 534.2 psi @Treatment Temp. 302 °F, Time 70.0 hour |
| 4.365 MPa @Treatment Temp. 275 °C, Time 252000 sec | 633.1 psi @Treatment Temp. 527 °F, Time 70.0 hour |
| 4.586 MPa @Treatment Temp. 23.0 °C, Time 252000 sec | 665.1 psi @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 4.602 MPa @Treatment Temp. 250 °C, Time 252000 sec | 667.4 psi @Treatment Temp. 482 °F, Time 70.0 hour |
| 4.714 MPa @Treatment Temp. 100 °C, Time 252000 sec | 683.7 psi @Treatment Temp. 212 °F, Time 70.0 hour |
| 4.93 MPa @Treatment Temp. 125 °C, Time 252000 sec | 715 psi @Treatment Temp. 257 °F, Time 70.0 hour |
| 5.032 MPa @Treatment Temp. 125 °C, Time 252000 sec | 729.9 psi @Treatment Temp. 257 °F, Time 70.0 hour |
Elongation, Ultimate | 279 % | 279 % |
| 167.1 % @Treatment Temp. 23.0 °C, Time 252000 sec | 167.1 % @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 200.3 % @Treatment Temp. 150 °C, Time 252000 sec | 200.3 % @Treatment Temp. 302 °F, Time 70.0 hour |
| 209 % @Treatment Temp. 200 °C, Time 252000 sec | 209 % @Treatment Temp. 392 °F, Time 70.0 hour |
| 238 % @Treatment Temp. 250 °C, Time 252000 sec | 238 % @Treatment Temp. 482 °F, Time 70.0 hour |
| 241.9 % @Treatment Temp. 275 °C, Time 252000 sec | 241.9 % @Treatment Temp. 527 °F, Time 70.0 hour |
| 255.1 % @Treatment Temp. 23.0 °C, Time 252000 sec | 255.1 % @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 267.1 % @Treatment Temp. 125 °C, Time 252000 sec | 267.1 % @Treatment Temp. 257 °F, Time 70.0 hour |
| 267.1 % @Treatment Temp. 125 °C, Time 252000 sec | 267.1 % @Treatment Temp. 257 °F, Time 70.0 hour |
| 287.9 % @Treatment Temp. 100 °C, Time 252000 sec | 287.9 % @Treatment Temp. 212 °F, Time 70.0 hour |
100% Modulus | 1.32 MPa | 192 psi |
Tear Strength | 10.9 kN/m | 62.0 pli |
Compression Set | 7.7 % @Treatment Temp. 200 °C, Time 79200 sec | 7.7 % @Treatment Temp. 392 °F, Time 22.0 hour |
| 9.2 % @Treatment Temp. 23.0 °C, Time 79200 sec | 9.2 % @Treatment Temp. 73.4 °F, Time 22.0 hour |
| 9.2 % @Treatment Temp. 175 °C, Time 79200 sec | 9.2 % @Treatment Temp. 347 °F, Time 22.0 hour |
|
Thermal Properties | Metric | English | Comments |
---|
Brittleness Temperature | -27.2 °C | -17.0 °F |
Shrinkage | -2.30 % @Treatment Temp. 150 °C, Time 252000 sec | -2.30 % @Treatment Temp. 302 °F, Time 70.0 hour |
| -1.70 % @Treatment Temp. 125 °C, Time 252000 sec | -1.70 % @Treatment Temp. 257 °F, Time 70.0 hour |
| 0.20 % @Treatment Temp. 125 °C, Time 252000 sec | 0.20 % @Treatment Temp. 257 °F, Time 70.0 hour |
| 0.20 % @Treatment Temp. 23.0 °C, Time 252000 sec | 0.20 % @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 0.60 % @Treatment Temp. 100 °C, Time 252000 sec | 0.60 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 1.8 % @Treatment Temp. 125 °C, Time 252000 sec | 1.8 % @Treatment Temp. 257 °F, Time 70.0 hour |
| 5.9 % @Treatment Temp. 23.0 °C, Time 252000 sec | 5.9 % @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 12.1 % @Treatment Temp. 150 °C, Time 252000 sec | 12.1 % @Treatment Temp. 302 °F, Time 70.0 hour |
| 21.8 % @Treatment Temp. 200 °C, Time 252000 sec | 21.8 % @Treatment Temp. 392 °F, Time 70.0 hour |
|
Descriptive Properties |
---|
Color | Black |