MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Aluminum Bronze D, UNS C61400, Annealed Rod
Categories: Metal; Nonferrous Metal; Copper Alloy; Bronze

Material Notes: Good to excellent corrosion resistance. Good hot and cold formability.

Applications: nuts, bolts, stringers and threaded members, corrosion resistant vessels and tanks, structural components, machine parts, condenser tube and piping systems, marine protective sheathing and fasteners, munitions mixing troughs and blending chambers.

Key Words: CDA 614
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.89 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 50
@Load 3000 kg,
Temperature 538 °C
 84
@Load 3000 kg,
Temperature 427 °C
 134
@Load 3000 kg,
Temperature 316 °C
 142
@Load 3000 kg,
Temperature 204 °C
 155
@Load 3000 kg,
Temperature 20.0 °C
 161
@Load 3000 kg,
Temperature -29.0 °C
 162
@Load 3000 kg,
Temperature -60.0 °C
 185
@Load 3000 kg,
Temperature -182 °C
Tensile Strength, Ultimate 92.0 MPa
@Temperature 538 °C
 174 MPa
@Temperature 427 °C
 427 MPa
@Temperature 316 °C
 522 MPa
@Temperature 204 °C
 583 MPa
@Temperature 20.0 °C
 600 MPa
@Temperature -29.0 °C
 610 MPa
@Temperature -60.0 °C
 707 MPa
@Temperature -182 °C
Tensile Strength, Yield 68.0 MPa
@Strain 0.5 %,
Temperature 538 °C
 123 MPa
@Strain 0.5 %,
Temperature 427 °C
 256 MPa
@Strain 0.5 %,
Temperature 316 °C
 276 MPa
@Strain 0.5 %,
Temperature 204 °C
 288 MPa
@Strain 0.5 %,
Temperature 20.0 °C
 303 MPa
@Strain 0.5 %,
Temperature -29.0 °C
 305 MPa
@Strain 0.5 %,
Temperature -60.0 °C
 347 MPa
@Strain 0.5 %,
Temperature -182 °C
Elongation at Break 30 %
@Temperature 316 °C
 34 %
@Temperature 204 °C
 36 %
@Temperature 538 °C
 44 %
@Temperature -29.0 °C
 45 %
@Temperature 20.0 °C
 47 %
@Temperature -60.0 °C
 52 %
@Temperature -182 °C
 60 %
@Temperature 427 °C
Reduction of Area 27 %
@Temperature 316 °C
 32 %
@Temperature 204 °C
 33 %
@Temperature 538 °C
 51 %
@Temperature -182 °C
 55 %
@Temperature 427 °C
 56 %
@Temperature -29.0 °C
 56 %
@Temperature 20.0 °C
 57 %
@Temperature -60.0 °C
Modulus of Elasticity 115 GPa
 45.0 GPa
@Temperature 538 °C
 67.0 GPa
@Temperature 427 °C
 81.0 GPa
@Temperature 316 °C
 130 GPa
@Temperature 204 °C
 136.5 GPa
@Temperature 20.0 °C
 139 GPa
@Temperature -182 °C
 172 GPa
@Temperature -29.0 °C
 176.5 GPa
@Temperature -60.0 °C
Poissons Ratio 0.312
Machinability 20 %UNS C36000 (free-cutting brass) = 100%
Shear Modulus 44.0 GPa
Charpy Impact 81.0 - 88.0 JKeyhole, temper not reported
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000123 ohm-cm
@Temperature 20.0 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 16.2 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.375 J/g-°C
Thermal Conductivity 56.5 W/m-K
Melting Point 1040 - 1045 °C
Solidus 1040 °C
Liquidus 1045 °C
Annealing Point 1125 - 1650 °F
 
Processing PropertiesOriginal ValueComments
Processing Temperature 1010 °CHot-Shortness Temperature
Annealing Temperature 600 - 900 °C
Hot-Working Temperature 800 - 925 °C
Recrystallization Temperature 785 - 870 °C
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 6.0 - 8.0 %
Copper, Cu 88 - 92.5 %
Iron, Fe 1.5 - 3.5 %
Lead, Pb <= 0.010 %
Manganese, Mn <= 1.0 %
Other, total <= 0.50 %
Phosphorus, P <= 0.015 %
Zinc, Zn <= 0.20 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum Bronze, UNS C61300, Annealed
Nickel Aluminum Bronze, UNS C63000, HR50 Temper
8% Aluminum Bronze, UNS C61000
Aluminum bronze 5%, UNS C60800
Ampco Metal AMPCO® 45 Nickel-Aluminum Bronze, Extruded and Drawn Rods, ≤ 25.4 mm.

MC61400c8 / 171644

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.