Envalior Pocan® KU 1-7301 000000 PBT
Categories:
Polymer
;
Thermoplastic
;
Polyester, TP
;
Polybutylene Terephthalate (PBT)
;
Polybutylene Terephthalate (PBT), Unreinforced, Molded
Material Notes:
PBT, non-reinforced, approved for food contact, Improved flowability
Former Lanxess product line is now with Envalior.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
1.31
g/cc
0.0473
lb/in³
ISO 1183
Linear Mold Shrinkage, Flow
0.018
cm/cm
0.018
in/in
Plaque 60 x 60 x 2mm; ISO 294-4
Linear Mold Shrinkage, Transverse
0.018
cm/cm
0.018
in/in
Plaque 60 x 60 x 2mm; ISO 294-4
Melt Flow
60
g/10 min
@Load 2.16 kg,
Temperature 260 °C
60
g/10 min
@Load 4.76 lb,
Temperature 500 °F
ISO 1133
Mechanical Properties
Metric
English
Comments
Tensile Strength, Yield
60.0
MPa
8700
psi
50 mm/min; ISO 527-1,-2
Elongation at Break
>= 10 %
>= 10 %
Nominal, 50 mm/min; ISO 527-1,-2
Elongation at Yield
9.0 %
9.0 %
50 mm/min; ISO 527-1,-2
Tensile Modulus
2.70
GPa
392
ksi
1 mm/min; ISO 527-1,-2
Flexural Yield Strength
80.0
MPa
@Strain 3.5 %
11600
psi
@Strain 3.5 %
2 mm/min; ISO 178-A
Flexural Strain at Yield
6.0 %
6.0 %
2 mm/min; ISO 178-A
Izod Impact, Notched (ISO)
<=
10.0
kJ/m²
@Temperature 23.0 °C
<=
4.76
ft-lb/in²
@Temperature 73.4 °F
ISO 180-1A
<=
10.0
kJ/m²
@Temperature -30.0 °C
<=
4.76
ft-lb/in²
@Temperature -22.0 °F
ISO 180-1A
Izod Impact, Unnotched (ISO)
90.0
kJ/m²
@Temperature -30.0 °C
42.8
ft-lb/in²
@Temperature -22.0 °F
ISO 180-1U
125
kJ/m²
@Temperature 23.0 °C
59.5
ft-lb/in²
@Temperature 73.4 °F
ISO 180-1U
Charpy Impact Unnotched
15.0
J/cm²
@Temperature -30.0 °C
71.4
ft-lb/in²
@Temperature -22.0 °F
ISO 179-1eU
18.0
J/cm²
@Temperature 23.0 °C
85.7
ft-lb/in²
@Temperature 73.4 °F
ISO 179-1eU
Charpy Impact, Notched
<=
1.00
J/cm²
@Temperature 23.0 °C
<=
4.76
ft-lb/in²
@Temperature 73.4 °F
ISO 179-1eA
<=
1.00
J/cm²
@Temperature -30.0 °C
<=
4.76
ft-lb/in²
@Temperature -22.0 °F
ISO 179-1eA
Electrical Properties
Metric
English
Comments
Volume Resistivity
>=
1.00e+13
ohm-cm
>=
1.00e+13
ohm-cm
IEC 60093
Surface Resistance
>=
1.00e+15
ohm
>=
1.00e+15
ohm
IEC 60093
Dielectric Constant
3.2
@Frequency 1e+6 Hz
3.2
@Frequency 1e+6 Hz
IEC 60250
Dissipation Factor
0.019
@Frequency 1e+6 Hz
0.019
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index
600
V
600
V
Test solution A; IEC 60112
Thermal Properties
Metric
English
Comments
CTE, linear, Parallel to Flow
110
µm/m-°C
@Temperature 23.0 - 55.0 °C
61.1
µin/in-°F
@Temperature 73.4 - 131 °F
ISO 11359-1,-2
CTE, linear, Transverse to Flow
110
µm/m-°C
@Temperature 23.0 - 55.0 °C
61.1
µin/in-°F
@Temperature 73.4 - 131 °F
ISO 11359-1,-2
Melting Point
225
°C
437
°F
10°C/min; ISO 11357-1,-3
Deflection Temperature at 0.46 MPa (66 psi)
65.0
°C
149
°F
Method Af; ISO 75-1,-2
Deflection Temperature at 1.8 MPa (264 psi)
140
°C
284
°F
Method Bf; ISO 75-1,-2
Flammability, UL94
HB
@Thickness 0.750 mm
HB
@Thickness 0.0295 in
UL Yellow Card
Glow Wire Flammability Index
750
°C
@Thickness 2.00 mm
1380
°F
@Thickness 0.0787 in
IEC 60695-2-12
Shrinkage, MD
0.30 %
@Treatment Temp. 120 °C,
Time 14400 sec
0.30 %
@Treatment Temp. 248 °F,
Time 4.00 hour
Flow Direction Post-Molding, Plaque 60 x 60 x 2mm; ISO 294-4
Shrinkage, TD
0.30 %
@Treatment Temp. 120 °C,
Time 14400 sec
0.30 %
@Treatment Temp. 248 °F,
Time 4.00 hour
Post-Molding, Plaque 60 x 60 x 2mm; ISO 294-4
Processing Properties
Metric
English
Comments
Melt Temperature
260
°C
500
°F
Plaque 60 x 60 x 2mm
Mold Temperature
80.0
°C
176
°F
Plaque 60 x 60 x 2mm
Hold Pressure
60.0
MPa
8700
psi
Plaque 60 x 60 x 2mm
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
PLANW9007 / 208448
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.