MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Teknor Apex Monprene® OM-10165 Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes: Notes: Monprene OM-10165 is a specialty thermoplastic elastomer, available in NAT, BLK, and colors, designed for overmolding applications like grips and anti-skid parts for a variety of consumer and industrial products. Monprene OM-10165is a medium hardness, low density opaque grade that exhibits excellent adhesion to nylon.

Availability: Africa & Middle East; Europe; Asia Pacific; Latin America; North America

Features: Abrasion Resistant; Bondability; Chemical Resistant; Chemically Coupled; Good Adhesion; Good Colorabillity; Good Moldability; Good Toughness; Low Density; Low Specific Gravity; Medium Flow; Medium Hardness; Slip; Soft; Sunlight Resistant; Weather Resistant; Without Fillers

Uses: Appliances; Bonding; Cell Phones; Flexible Grips; Handles; Industrial Applications; Knobs; Overmolding; Power/Other Tools; Rubber Replacement; Sporting Goods; Writing Instruments

RoHS Compliance: RoHS Compliant

Form: Pellets

Processing Method: Injection Molding

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.920 g/cc0.0332 lb/in³ASTM D792
Melt Flow 8.0 g/10 min
@Load 2.16 kg,
Temperature 190 °C
8.0 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A  65
@Time 5.00 sec
65
@Time 0.00139 hour
Injection Molded; ASTM D2240
 67
@Time 1.00 sec
67
@Time 0.000278 hour
Injection Molded; ASTM D2240
Tensile Strength at Break 5.32 MPa771 psi20 in/min, Across Flow; ASTM D412
 5.50 MPa798 psi20 in/min, Flow; ASTM D412
Tensile Stress at Strain  2.32 MPa
@Strain 100 %
337 psi
@Strain 100 %
20 in/min, Across Flow; ASTM D412
 3.04 MPa
@Strain 100 %
441 psi
@Strain 100 %
20 in/min, Flow; ASTM D412
 3.67 MPa
@Strain 300 %
533 psi
@Strain 300 %
20 in/min, Across Flow; ASTM D412
 4.81 MPa
@Strain 300 %
697 psi
@Strain 300 %
20 in/min, Flow; ASTM D412
Elongation at Break 440 %440 %20 in/min, Flow; ASTM D412
 520 %520 %20 in/min, Across Flow; ASTM D412
Tear Strength 29.3 kN/m167 pli20 in/min, Across Flow; ASTM D624
 30.7 kN/m175 pli20 in/min, Flow; ASTM D624
Compression Set 29 %
@Temperature 22.8 °C,
Time 79200 sec
29 %
@Temperature 73.0 °F,
Time 22.0 hour
Type 1; ASTM D395B
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 204 - 232 °C400 - 450 °F
Middle Barrel Temperature 227 - 249 °C440 - 480 °F
Front Barrel Temperature 249 - 266 °C480 - 510 °F
Nozzle Temperature 266 - 277 °C510 - 530 °F
Melt Temperature 266 - 277 °C510 - 530 °F
Mold Temperature 23.9 - 60.0 °C75.0 - 140 °F
Injection Pressure 1.38 - 6.89 MPa200 - 1000 psi
Back Pressure 0.172 - 0.862 MPa25.0 - 125 psi
Cushion 0.381 - 2.54 cm0.150 - 1.00 in
Screw Speed 50 - 120 rpm50 - 120 rpm
 
Descriptive Properties
AppearanceBlack
 Colors Available
 Grey
 Natural Color
 Opaque

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PTEKNQ0890 / 237381

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.