MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Assab Steels ASSAB 88 Cold Work Steel
Categories: Metal; Ferrous Metal; Chrome-moly Steel; Tool Steel; Cold Work Steel

Material Notes: ASSAB 88 (SLEIPNER) is a chromium-molybdenum-vanadium alloyed tool steel which is characterized by:
  • Good wear resistance
  • Good chipping resistance
  • High compressive strength
  • High hardness (>60HRC) after high temperature tempering
  • Good through-hardening properties
  • Good stability in hardening
  • Good resistance to tempering back
  • Good WEDM properties
  • Good machinability and grindability
  • Good surface treatment properties

ASSAB 88 (SLEIPNER) is a general purpose steel for cold work tooling. ASSAB 88 (SLEIPNER) is recommended for medium run tooling applications. Examples:

  • Blanking and fine blanking
  • Shearing
  • Forming
  • Coining
  • Cold forging
  • Cold extrusion
  • Thread rolling
  • Drawing and deep drawing
  • Powder pressing

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.279 lb/in³
 0.275 lb/in³
@Temperature 400 °C
 0.277 lb/in³
@Temperature 200 °C
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell C 551075°C Austenitizing temperature, for tempering at 400°C
 561075°C Austenitizing temperature, for tempering at 250°C
 581050°C Austenitizing temperature, for tempering at 400°C
 591030°C Austenitizing temperature, for tempering at 250°C
 591050°C Austenitizing temperature, for tempering at 250°C
 601030°C Austenitizing temperature, for tempering at 400°C
 601030°C Austenitizing temperature, for tempering at 550°C
 611050°C Austenitizing temperature, for tempering at 550°C
 62Hardened and tempered.
 62.5At 1075°C Austenitizing temperature (30 min)
 631075°C Austenitizing temperature, for tempering at 550°C
 64.25At 1000°C Austenitizing temperature (30 min)
 64.5At 1035°C Austenitizing temperature (30 min)
Modulus of Elasticity 205 GPa
 180 GPa
@Temperature 400 °C
Compressive Yield Strength 2050 MPaapproximate, Hardness HRC 55 Rc0.2
 2500 MPaapproximate, Hardness HRC 62 Rc0.2
 
Thermal PropertiesOriginal ValueComments
CTE, linear 11.6 µm/m-°C
@Temperature 20.0 - 200 °C
after high temperature tempering
 12.4 µm/m-°C
@Temperature 20.0 - 400 °C
after high temperature tempering
 12.7 µm/m-°C
@Temperature 20.0 - 200 °C
after low temperature tempering (60 HRC)
Specific Heat Capacity 0.110 BTU/lb-°F
@Temperature 20.0 °C
Thermal Conductivity 20.0 W/m-K
@Temperature 200 °C
 25.0 W/m-K
@Temperature 400 °C
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.90 %
Chromium, Cr 7.8 %
Iron, Fe 86.9 %
Manganese, Mn 0.50 %
Molybdenum, Mo 2.5 %
Silicon, Si 0.90 %
Vanadium, V 0.50 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Chrome-moly Steel
Assab Steels ASSAB XW-42 Cold Work Steel
ASTM A182, Grade F11, Class 1
Assab Steels ASSAB XW-41 Cold Work Steel
Assab Steels VANADIS 4 Cold Work Steel

NASSAB01 / 15019

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.