MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Refractory Metals

(Viewing data as-entered. Click here to return)
Mo-47.5 Re Molybdenum Rhenium Alloy, Annealed
Categories: Metal; Nonferrous Metal; Molybdenum Alloy; Refractory Metal

Material Notes: Annealed applies only to tensile; other property values are typical of this alloy. Ductile to brittle transition temperature (DBBT) (-273) - (-173) °C. Stress relieving temperature 1000-1200°C. Recrystallization Temperature 1300-1550°C. Bcc crystal lattice.

Key Words: Rhenium Molybdenum Alloys
Vendors: Elmet Technologies is a 100% US owned and operated, fully integrated manufacturer of Molybdenum, Tungsten and related alloys such as TZM, WHA & MoLa. At our 220,000 sqr/ft plant in Lewiston, Maine, Elmet manufactures W & Mo pure powders plus rod, wire, plate, sheet & foil in additional to offering fabrication and machining services. ITAR, ISO and AS9100 registered. www.elmettechnologies.com

PLANSEE SE: Whether it's high temperatures, aggressive chemicals or extreme mechanical loading: PLANSEE supplies a suitable product solution in refractory metals or composite materials. As the world market leader in powder metallurgically produced high performance materials we combine outstanding materials knowledge with profound applications and technology know-how. Visit us at www.plansee.com.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 13.5 g/cc
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 1180 MPaVacuum-melted
 240 MPa
@Temperature 1200 °C
Vacuum-melted prior to test
 620 MPa
@Temperature 800 °C
Vacuum-melted prior to test
Tensile Strength, Yield 845 MPa
 210 MPa
@Temperature 1200 °C
 415 MPa
@Temperature 800 °C
Elongation at Break 22 %
Modulus of Elasticity 365 GPa
Poissons Ratio 0.285
Shear Modulus 132 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000220 ohm-cmTemp Coefficient is 0.0017/°C 20-1000°C.
Critical Superconducting Temperature 10.9 K
 
Thermal PropertiesOriginal ValueComments
CTE, linear 5.72 µm/m-°C
@Temperature 500 °C
 6.45 µm/m-°C
@Temperature 1000 °C
Thermal Conductivity 36.8 W/m-K
Melting Point 2450 °C
Maximum Service Temperature, Air 725 °Csharp increase in oxidation
 
Component Elements PropertiesOriginal ValueComments
Molybdenum, Mo 52.5 %
Rhenium, Re 47.5 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Mo-47.5 Re Molybdenum Rhenium Alloy, Deformed
Mo-44.5 Re Molybdenum Rhenium Alloy, Annealed
Mo-30Re Molybdenum Rhenium Alloy, Stress Relief Annealed
Plansee MoRe41 Molybdenum-Rhenium
Plansee MoRe5 Molybdenum-Rhenium

MRMo31 / 13896

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.