MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Toyobo Celstran® PPS-GF40-02 AD3002 Black PPS, 40% Long Glass Reinforced
Categories: Polymer; Thermoplastic; Polyphenylene Sulfide (PPS); Polyphenylene Sulfide (PPS) with 40% Glass Fiber Filler

Material Notes: Product Description: 40% long strand fiber glass reinforced polyphenylene sulfide

Availability: Africa & Middle East; Europe; Asia Pacific; Latin America; North America

Filler/Reinforcement: Glass Fiber

Form: Pellets

Processing Method: Injection Molding

Information provided by Celanese

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.65 g/cc0.0596 lb/in³ISO 1183
Maximum Moisture Content 0.0200.020
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 165 MPa23900 psiISO 527-2/5
Elongation at Break 1.3 %1.3 %ISO 527-2/5
Tensile Modulus 14.8 GPa2150 ksiISO 527-1
Flexural Strength 265 MPa38400 psiISO 178
Flexural Modulus 14.3 GPa2070 ksiISO 178
Charpy Impact Unnotched 3.99 J/cm²19.0 ft-lb/in²ISO 179/1eU
Charpy Impact, Notched 2.31 J/cm²11.0 ft-lb/in²ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 1.8 MPa (264 psi) 270 °C518 °FUnannealed; ISO 75-2/A
Deflection Temperature at 8.0 MPa 240 °C464 °FUnannealed; ISO 75-2/C
 
Processing PropertiesMetricEnglishComments
Processing Temperature 70.0 - 80.0 °C158 - 176 °FHopper
Feed Temperature 20.0 - 50.0 °C68.0 - 122 °FInjection
Rear Barrel Temperature 285 - 295 °C545 - 563 °F
Middle Barrel Temperature 290 - 300 °C554 - 572 °F
Front Barrel Temperature 295 - 305 °C563 - 581 °F
Nozzle Temperature 290 - 300 °C554 - 572 °F
Zone 4 300 - 310 °C572 - 590 °FInjection
Melt Temperature 300 - 315 °C572 - 599 °F
Mold Temperature 140 - 160 °C284 - 320 °F
Drying Temperature 130 - 140 °C266 - 284 °F
Dry Time 3.00 - 4.00 hour3.00 - 4.00 hour

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PHCQ6260 / 310953

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.