MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Mocom (ALBIS) ALCOM® PC 740/4.2 UV WT1217-10LD3 PC
Categories: Polymer; Thermoplastic; Polycarbonate (PC)

Material Notes: Base Polymer: Polycarbonate

Filler/Additive System: Special filler

Special Features: Light scattering, high light diffusion

Market Segment: Automotive, Lighting

Application Area: Lighting, light transparent components

Typical Applications: Lamp covers, display elements, operating elements

Information provided by Albis Plastics

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.19 g/cc0.0430 lb/in³ISO 1183
Maximum Moisture Content 0.0200.020
Linear Mold Shrinkage 0.0060 - 0.0080 cm/cm
@Time 86400 sec
0.0060 - 0.0080 in/in
@Time 24.0 hour
ISO 294-4
Melt Flow 17 g/10 min
@Load 1.20 kg,
Temperature 300 °C
17 g/10 min
@Load 2.65 lb,
Temperature 572 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 64.0 MPa9280 psiISO 527
Tensile Strength, Yield 63.0 MPa9140 psiISO 527
Elongation at Break 90 %90 %ISO 527
Elongation at Yield 6.0 %6.0 %ISO 527
Tensile Modulus 2.30 GPa334 ksiISO 527
Flexural Strength 95.0 MPa13800 psiISO 178
 74.0 MPa
@Strain 3.5 %
10700 psi
@Strain 3.5 %
ISO 178
Flexural Modulus 2.40 GPa348 ksiISO 178
Charpy Impact Unnotched  NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
ISO 179/1eU
 NB
@Temperature -40.0 °C
NB
@Temperature -40.0 °F
ISO 179/1eU
Charpy Impact, Notched  1.10 J/cm²
@Temperature -40.0 °C
5.23 ft-lb/in²
@Temperature -40.0 °F
ISO 179/1eA
 1.20 J/cm²
@Temperature 23.0 °C
5.71 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 1.8 MPa (264 psi) 128 °C262 °FISO 75-1/-2
Vicat Softening Point 142 °C288 °FB50; ISO 306
Flammability, UL94  HB
@Thickness 1.50 mm
HB
@Thickness 0.0591 in
 V-2
@Thickness 0.750 mm
V-2
@Thickness 0.0295 in
Glow Wire Flammability Index  850 °C
@Thickness 1.00 mm
1560 °F
@Thickness 0.0394 in
passed; DIN EN 60695
 850 °C
@Thickness 2.00 mm
1560 °F
@Thickness 0.0787 in
passed; DIN EN 60695
 850 °C
@Thickness 3.00 mm
1560 °F
@Thickness 0.118 in
passed; DIN EN 60695
 850 °C
@Thickness 4.00 mm
1560 °F
@Thickness 0.157 in
passed; DIN EN 60695
 960 °C
@Thickness 3.00 mm
1760 °F
@Thickness 0.118 in
passed; DIN EN 60695
 960 °C
@Thickness 4.00 mm
1760 °F
@Thickness 0.157 in
passed; DIN EN 60695
 
Optical PropertiesMetricEnglishComments
Haze 95 %
@Thickness 1.00 mm
95 %
@Thickness 0.0394 in
A,2°; ISO 13468
Transmission, Visible 16 %
@Thickness 1.00 mm
16 %
@Thickness 0.0394 in
A,2°; ISO 13468
 
Processing PropertiesMetricEnglishComments
Melt Temperature 270 - 310 °C518 - 590 °FInjection molding
Mold Temperature 80.0 - 110 °C176 - 230 °FInjection molding
Drying Temperature  100 - 120 °C
@Time 14400 - 43200 sec
212 - 248 °F
@Time 4.00 - 12.0 hour
in air circulating dryer
 120 °C
@Time 7200 - 10800 sec
248 °F
@Time 2.00 - 3.00 hour
in a dry air (desiccant) dryer
 
Descriptive Properties
Base PolymerPolycarbonate
Half Power Angle57°d=1mm, A,2°

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PALBIS8181 / 242240

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.