MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Extreme Materials from MCAM
Visit Mitsubishi Chemical Advanced Materials for Extreme Materials - high performance plastic machining stock engineered to replace metals such as nickel alloys or stainless steel.

Kennametal Stellite Deloro® 208 PM cast
Categories: Metal; Nonferrous Metal; Nickel Alloy; Superalloy

Material Notes: Adhesive wear test data: cast 0.06 Typical applications include vane plugs, fuel metering pins, spacer bushings, ball bearing blanks, race bearing blanks, diesel engine exhaust, fluid valve seats, saw cutter inserts, miscellaneous wear parts. Data provided by the manufacturer, Deloro Stellite Inc.

Product of former Deloro Stellite Inc.

Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 8.40 g/cc0.303 lb/in³P/M (98%)
 8.53 g/cc0.308 lb/in³Theoretical
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 676 MPa98000 psi
 547 MPa
@Temperature 538 °C
79300 psi
@Temperature 1000 °F
 626 MPa
@Temperature 760 °C
90800 psi
@Temperature 1400 °F
 652 MPa
@Temperature 649 °C
94600 psi
@Temperature 1200 °F
Elongation at Break <= 1.0 %<= 1.0 %in 25.4 mm
 <= 1.0 %
@Temperature 538 °C
<= 1.0 %
@Temperature 1000 °F
in 25.4 mm
 <= 1.0 %
@Temperature 649 °C
<= 1.0 %
@Temperature 1200 °F
in 25.4 mm
 
Component Elements PropertiesMetricEnglishComments
Boron, B <= 1.0 %<= 1.0 %
Carbon, C 2.6 %2.6 %
Chromium, Cr 26 %26 %
Cobalt, Co 10 %10 %
Iron, Fe 12.5 %12.5 %
Manganese, Mn <= 0.75 %<= 0.75 %
Molybdenum, Mo 10 %10 %
Nickel, Ni 24 %24 %As Remainder
Phosphorus, P <= 0.040 %<= 0.040 %
Silicon, Si <= 1.0 %<= 1.0 %
Sulfur, S <= 0.030 %<= 0.030 %
Tungsten, W 10 %10 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Kennametal Stellite Deloro® 716 PM cast
Kennametal Stellite Stellite® 31 PM cast
Kennametal Stellite Deloro® 208 PM after P/M Processing
Kennametal Stellite Deloro® 711 PM cast
Kennametal Stellite Deloro® N-6 PM with P/M Processing

ND208B / 16076

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.