BASF Ultramid® B3U Q721 Nylon 6
Categories:
Polymer
;
Thermoplastic
;
Nylon (Polyamide PA)
;
Nylon 6 (PA6)
;
Nylon 6, Unreinforced
Material Notes:
Ultramid B3U Q721 is an injection molding grade, flame-retardant, free from halogen and phosphorus, and UL94 V0 approved. Technical molded parts are used for electrical engineering.
Information provided by BASF.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
1.17
g/cc
0.0423
lb/in³
ISO 1183
Moisture Absorption
2.50 %
2.50 %
50% RH; ISO 62
Water Absorption at Saturation
9.5 %
9.5 %
ISO 62
Mechanical Properties
Metric
English
Comments
Tensile Strength at Break
74.0
MPa
10700
psi
Dry; ISO 527
Tensile Strength, Yield
45.0
MPa
6530
psi
Conditioned; ISO 527
80.0
MPa
11600
psi
Dry; ISO 527
Elongation at Break
6.4 %
6.4 %
Dry; ISO 527
Elongation at Yield
4.0 %
4.0 %
Dry; ISO 527
15 %
15 %
Conditioned; ISO 527
Tensile Modulus
1.10
GPa
160
ksi
Conditioned; ISO 527
3.70
GPa
537
ksi
Dry; ISO 527
Flexural Modulus
3.00
GPa
435
ksi
Dry; ISO 178
Charpy Impact Unnotched
NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
Conditioned; ISO 179
NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
Dry; ISO 179
Charpy Impact, Notched
0.300
J/cm²
@Temperature -30.0 °C
1.43
ft-lb/in²
@Temperature -22.0 °F
Dry; ISO 179
0.300
J/cm²
@Temperature 23.0 °C
1.43
ft-lb/in²
@Temperature 73.4 °F
Dry; ISO 179
Electrical Properties
Metric
English
Comments
Volume Resistivity
1.00e+10
ohm-cm
1.00e+10
ohm-cm
Conditioned; IEC 60093
1.00e+13
ohm-cm
1.00e+13
ohm-cm
Dry; IEC 60093
Dielectric Constant
3.4
@Frequency 1e+6 Hz
3.4
@Frequency 1e+6 Hz
Dry; IEC 60250
6.0
@Frequency 1e+6 Hz
6.0
@Frequency 1e+6 Hz
Conditioned; IEC 60250
Dissipation Factor
0.015
@Frequency 1e+6 Hz
0.015
@Frequency 1e+6 Hz
Dry; IEC 60250
0.25
@Frequency 1e+6 Hz
0.25
@Frequency 1e+6 Hz
Conditioned; IEC 60250
Comparative Tracking Index
600
V
600
V
Dry; IEC 60112
Thermal Properties
Metric
English
Comments
Melting Point
220
°C
428
°F
ISO 3146
Deflection Temperature at 0.46 MPa (66 psi)
190
°C
374
°F
ISO 75
Deflection Temperature at 1.8 MPa (264 psi)
65.0
°C
149
°F
ISO 75
UL RTI, Electrical
130
°C
@Thickness 0.750 mm
266
°F
@Thickness 0.0295 in
UL746B
130
°C
@Thickness 1.50 mm
266
°F
@Thickness 0.0591 in
UL746B
130
°C
@Thickness 3.00 mm
266
°F
@Thickness 0.118 in
UL746B
UL RTI, Mechanical with Impact
75.0
°C
@Thickness 0.750 mm
167
°F
@Thickness 0.0295 in
UL746B
75.0
°C
@Thickness 1.50 mm
167
°F
@Thickness 0.0591 in
UL746B
80.0
°C
@Thickness 3.00 mm
176
°F
@Thickness 0.118 in
UL746B
UL RTI, Mechanical without Impact
95.0
°C
@Thickness 0.750 mm
203
°F
@Thickness 0.0295 in
UL746B
95.0
°C
@Thickness 1.50 mm
203
°F
@Thickness 0.0591 in
UL746B
95.0
°C
@Thickness 3.00 mm
203
°F
@Thickness 0.118 in
UL746B
Flammability, UL94
V-0
@Thickness 0.750 mm
V-0
@Thickness 0.0295 in
V-0
@Thickness 1.50 mm
V-0
@Thickness 0.0591 in
V-0
@Thickness 3.00 mm
V-0
@Thickness 0.118 in
Processing Properties
Metric
English
Comments
Melt Temperature
240
-
285
°C
464
-
545
°F
Mold Temperature
65.0
-
80.0
°C
149
-
176
°F
Drying Temperature
80.0
°C
@Time 7200 - 14400 sec
176
°F
@Time 2.00 - 4.00 hour
Moisture Content
<= 0.15 %
<= 0.15 %
Injection Pressure
3.45
-
10.3
MPa
500
-
1500
psi
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
PBASF8963 / 254921
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.