MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Materion ToughMet® 3 CA  (discontinued **)
Categories: Metal; Nonferrous Metal; Copper Alloy

Material Notes: ToughMet® is Brush Wellman's solution for severe service material problems. By applying their EquaCast® process, tailored alloying additions and spinodal hardening technology, they have engineered ToughMet® to provide attributes beyond those typically found in a high-strength copper alloy.

  • Exceptional resistance to corrosion and cavitation
  • Outstanding lubricity and durability in demanding applications
  • Highly uniform composition in all product forms
  • Uniform microstructure in a variety of wrought shapes and sizes

ToughMet® 3 in the wrought and spinodally hardened (AT) condition exhibits tensile strength up to 140 ksi and hardness up to HRc 34 in a Copper-15% Nickel-8% Tin alloy with excellent machinability.

Information supplied by Brush Wellman Engineered Materials.

Brush Engineered Materials Inc. changed its name to Materion Corporation in March 2011.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.323 lb/in³
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell B 62 - 75
Tensile Strength, Ultimate 50000 - 75000 psi
Tensile Strength, Yield 20000 - 40000 psi
@Strain 0.2 %
Elongation at Break >= 30 %
Modulus of Elasticity 18500 ksi
Poissons Ratio 0.30
Shear Modulus 7120 ksicalculated
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000192 ohm-cmConductivity is 9% IACS
Magnetic Permeability <= 1.001
 
Thermal PropertiesOriginal ValueComments
CTE, linear 9.10 µin/in-°F
@Temperature 21.1 - 102 °C
Thermal Conductivity 264 BTU-in/hr-ft²-°F
 
Component Elements PropertiesOriginal ValueComments
Copper, Cu 77 %As remainder
Nickel, Ni 15 %
Tin, Sn 8.0 %

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Materion ToughMet® 3 AT110 (OD≥4")
Materion ToughMet® 2 CX 90
Materion ToughMet® 3 AT120 (OD≥4")
Materion ToughMet® 3 AT90 (OD≥4")
Materion ToughMet® 3 CX90

NBBC12 / 15322

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.