MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
SABIC LEXAN™ FR 945U PC (Asia)
Categories: Polymer; Thermoplastic; Polycarbonate (PC)

Material Notes: LEXAN 945U Polycarbonate (PC) is an injection moldable non-chlorinated/brominated, unfilled flame retardant grade with medium flow. It is UV stabilized and has an MVR of 10 (300°C/1.2kg) and a UL94 V0@1.5mm, and is available in various opaque color options.

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.19 g/ccASTM D792
Linear Mold Shrinkage, Flow 0.0060 - 0.0080 cm/cm
@Thickness 3.20 mm
SABIC method
Melt Flow 10 g/10 min
@Load 1.20 kg,
Temperature 300 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 65.0 MPa50 mm/min; ASTM D638
Tensile Strength, Yield 62.0 MPa50 mm/min; ASTM D638
Elongation at Break 125 %50 mm/min; ASTM D638
Elongation at Yield 6.0 %50 mm/min; ASTM D638
Tensile Modulus 2270 MPa50 mm/min; ASTM D638
Flexural Yield Strength 101 MPa1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 2340 MPa1.3 mm/min, 50 mm span; ASTM D790
Izod Impact, Notched 801 J/mASTM D256
Dart Drop, Total Energy 73.0 JASTM D3763
 
Electrical PropertiesOriginal ValueComments
Arc Resistance 0.00 - 60 secASTM D495
Comparative Tracking Index 175 - 250 VUL 746A
Hot Wire Ignition, HWI 30 - 60 secUL 746A
High Amp Arc Ignition, HAI 30 - 60 arcsUL 746A
High Voltage Arc-Tracking Rate, HVTR 80.0 - 150 mm/minUL 746A
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 66.6 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E831
CTE, linear, Transverse to Flow 66.6 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E831
Deflection Temperature at 0.46 MPa (66 psi) 137 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 126 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Vicat Softening Point 143 °CRate B/50; ASTM D1525
UL RTI, Electrical 130 °CUL 746B
UL RTI, Mechanical with Impact 120 °CUL 746B
UL RTI, Mechanical without Impact 130 °CUL 746B
Flammability, UL94 V-0
@Thickness 1.50 mm
UL 94
Glow Wire Test 800 °C
@Thickness 1.50 mm
IEC 60695-2-13
 960 °C
@Thickness 1.00 mm
IEC 60695-2-12
 
Processing PropertiesOriginal ValueComments
Nozzle Temperature 290 - 310 °CInjection Molding
Zone 1 270 - 295 °C
Zone 2 280 - 305 °C
Zone 3 295 - 315 °C
Melt Temperature 295 - 315 °C
Mold Temperature 70.0 - 95.0 °C
Drying Temperature 120 °CInjection Molding
Dry Time 3.00 - 4.00 hourInjection Molding
 48.0 hourCumulative; Injection Molding
Moisture Content 0.020 %
Back Pressure 0.300 - 0.700 MPa
Shot Size 40 - 60 %
Vent Depth 0.00250 - 0.00760 cm
Screw Speed 40 - 70 rpm
 
Descriptive Properties
UV-light, water exposure/immersionF1UL 746C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABI10619 / 244086

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.