MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

3M AC-350 Class C-8(24) Aerospace Sealant
Categories: Polymer; Thermoset; Polysulfide Sealant/Adhesive

Material Notes: 3M Aerospace Sealant AC-350 Class C are fast-cure, intermediate density polysulfide sealant suitable fro fuel tank and fuselage applications. These two-component, manganese dioxide cured sealant have resistance to aviation gasoline and jet fuel, as well as resistance to chemicals and petroleum products common to other aircraft industry. 3M AC-350 Class C Sealants maintain flexibility and bond strength on most metal substrates such as aluminum, titanium, steel, stainless steel, and many coatings under extremes of temperature, weathering and stress. The mixed compound is a flowable, faying surface grade material easily applied by brush, roller, spatula, or extrusion gun. The sealant exhibits good tooling properties.

Information provided by 3M

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density <= 1.40 g/cc<= 0.0506 lb/in³cured 14 days @ 50% RH
Volatiles 5.0 %5.0 %
Brookfield Viscosity 200000 - 350000 cP200000 - 350000 cPBase, RVF #7 sp @ 2 rpm
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 50 - 5550 - 55cured 14 days @ 50% RH
Shear Strength  1.65 MPa
@Time 1.21e+6 sec
240 psi
@Time 336 hour
Graphite Bismaleimide (BMI) composite IM7/5250-4
 1.86 MPa
@Time 346000 sec
270 psi
@Time 96.0 hour
AMS4911 Titanium
Peel Strength  6.49 kN/m
@Temperature 60.0 °C,
Time 605000 sec
37.0 pli
@Temperature 140 °F,
Time 168 hour
in JRF, Graphite/BMI
 6.66 kN/m
@Temperature 60.0 °C,
Time 605000 sec
38.0 pli
@Temperature 140 °F,
Time 168 hour
in JRF, MIL-C-27725
 6.84 kN/m
@Temperature 60.0 °C,
Time 605000 sec
39.0 pli
@Temperature 140 °F,
Time 168 hour
in JRF/SW, Graphite/BMI
 7.19 kN/m
@Temperature 60.0 °C,
Time 605000 sec
41.0 pli
@Temperature 140 °F,
Time 168 hour
in JRF, MIL-C-5541
 7.36 kN/m
@Temperature 60.0 °C,
Time 605000 sec
42.0 pli
@Temperature 140 °F,
Time 168 hour
in JRF/SW, MIL-C-27725
 7.36 kN/m
@Temperature 60.0 °C,
Time 605000 sec
42.0 pli
@Temperature 140 °F,
Time 168 hour
in JRF/SW, MIL-PRF-85582
 7.89 kN/m
@Temperature 60.0 °C,
Time 605000 sec
45.0 pli
@Temperature 140 °F,
Time 168 hour
in JRF/SW, MIL-C-5541
 7.89 kN/m
@Temperature 60.0 °C,
Time 605000 sec
45.0 pli
@Temperature 140 °F,
Time 168 hour
in JRF, AMS 4911 Titanium
 7.89 kN/m
@Temperature 60.0 °C,
Time 6.05e+6 sec
45.0 pli
@Temperature 140 °F,
Time 1680 hour
in JRF/SW, AMS 4911 Titanium
 7.89 kN/m
@Temperature 60.0 °C,
Time 605000 sec
45.0 pli
@Temperature 140 °F,
Time 168 hour
in JRF, MIL-PRF-85582
 8.24 kN/m
@Temperature 60.0 °C,
Time 605000 sec
47.0 pli
@Temperature 140 °F,
Time 168 hour
in JRF/SW, AMS 4911 Titanium
 9.99 kN/m
@Temperature 60.0 °C,
Time 6.05e+6 sec
57.0 pli
@Temperature 140 °F,
Time 1680 hour
in JRF, AMS 4911 Titanium
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 121 °C250 °Fcured 14 days @ 50% RH
 182 °C360 °FShort term, cured 14 days @ 50% RH
Minimum Service Temperature, Air -54.0 °C-65.2 °Fcured 14 days @ 50% RH
 
Processing PropertiesMetricEnglishComments
Cure Time 5760 min96.0 hour
Tack-Free Time 5760 min96.0 hour
Shelf Life 9.00 Month
@Temperature <=26.7 °C
9.00 Month
@Temperature <=80.1 °F
 
Descriptive Properties
AppearanceBrownAccelerator
 Dark Gray
 Off WhiteBase

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI 1015 Steel, as rolled

PMM35392 / 170139

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.