MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Arkema Rilsan® MB 3000 NAT Nylon 11, Sheathing Grade
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 11 (PA11); Nylon 11, Cable Sheathing Grade

Material Notes: Designation ISO 1874-PA11,MF,12-010

Polyvalent rigid grade for injection molding and sheathing of cables. Available color: natural. Flame retardant agent, halogen free. Fire-resistant. Easy to be processed for injection molding and sheathing of cables. Low shrinkage for molding: include 1% on average for the mold design.

UL classification: UL94 V0 (3mm) RTI(C) 65/65/65

Example applications: Electrical cables, all pieces with fireproofing required.

Information provided by Arkema.

Key Words: PA11; Polyamide 11
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.09 g/ccISO 1183
 1.09 g/ccCond.; ISO 1183
Water Absorption 2.0 %Dry; Sim. to ISO 62
Moisture Absorption 0.600 %Dry; Sim. to ISO 62
Linear Mold Shrinkage, Flow 0.0090 cm/cmDry; ISO 294-4, 2577
 0.0090 cm/cm
Melt Flow 95 g/10 min
@Load 2.16 kg,
Temperature 235 °C
cm³/10 min Volumetric Rate; ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 69
@Time 15.0 sec
Dry; ISO 7619-1
Tensile Strength, Yield 45.0 MPaDry; ISO 527-1/-2
 45.0 MPaCond.; ISO 527-1/-2
Elongation at Break >= 50 %Dry; ISO 527-1/-2
 >= 50 %Cond.; ISO 527-1/-2
Elongation at Yield 5.0 %Dry; ISO 527-1/-2
 5.0 %Cond.; ISO 527-1/-2
Tensile Modulus 1830 MPaCond.; ISO 527-1/-2
Charpy Impact Unnotched 38.0 kJ/m²
@Temperature -30.0 °C
Cond.; ISO 179/1eU
 83.0 kJ/m²
@Temperature 23.0 °C
Cond.; ISO 179/1eU
Charpy Impact, Notched 3.00 kJ/m²
@Temperature -30.0 °C
Cond.; ISO 179/1eA
 4.00 kJ/m²
@Temperature 23.0 °C
Cond.; ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+15 ohm-cm
 >= 1.00e+15 ohm-cm
Surface Resistance >= 1.00e+15 ohmCond.; IEC 60093
Dielectric Constant 3.0
@Frequency 1e+6 Hz
Dry; IEC 60250
 3.0
@Frequency 100 Hz
Dry; IEC 60250
Dielectric Strength 28.0 kV/mmDry; IEC 60243-1
 28.0 kV/mmCond.; IEC 60243-1
Dissipation Factor 0.018
@Frequency 1e+6 Hz
Dry; IEC 60250
 0.0221
@Frequency 100 Hz
Dry; IEC 60250
Comparative Tracking Index 600 VCond.; IEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 102 µm/m-°CDry; ISO 11359-1/-2
Melting Point 189 °C10°C/min; Dry; ISO 11357-1/-3
Flammability, UL94 V-0
@Thickness 0.800 mm
Yellow Card Available; Dry; IEC 60695-11-10
 V-0
@Thickness 1.60 mm
Yellow Card Available; Dry; IEC 60695-11-10
Oxygen Index 33 %Dry; ISO 4589-1/-2
 
Processing PropertiesOriginal ValueComments
Melt Temperature 260 °CInjection Molding; ISO 294
Mold Temperature 50.0 °CInjection Molding; ISO 10724
Hold Pressure 16.0 MPaInjection Molding; ISO 294
 
Descriptive Properties
%Bio-Based90ASTM D6866
Bio-BasedYes
Form as DeliveredPellets
Heat StabilizedYes
Light StabilizedYes
LubricantsYes
Moisture SensitiveYes
Processing MethodsInjection Molding

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Arkema Rilsan® BESNO P40 W6 TL PA11 FR(30)
Arkema Rilsan® BZM 30 O TL PA11-GF30
Clariant Renol PA113G30TF15S2 Nylon 66, 30% Glass Fiber, Teflon and Silicone Lubricated
EMS-Grivory Grilamid® TR 90 PAMACM12
Techmer ES Luriblend® PA11 GF30 TL20 LE 30% Glass Filled

PARKG661 / 25910

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.