MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Sandvik 5CR12 Plate, Sheet and Coil
Categories: Metal; Ferrous Metal; Alloy Steel; Ferritic

Material Notes: Sandvik 5CR12 is a Ferritic chromium-nickel steel.

Information provided by Sandvik

UNS S40977; EN 1.4003

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.70 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Vickers 160 - 170
Tensile Strength, Ultimate 450 - 650 MPa
Tensile Strength, Yield >= 280 MPaLongitudinal
 >= 280 MPaTransverse
 >= 215 MPa
@Strain 0.2 %,
Temperature 300 °C
 220 MPa
@Strain 0.2 %,
Temperature 250 °C
 220 MPa
@Strain 0.2 %,
Temperature 250 °C
 230 MPa
@Strain 0.2 %,
Temperature 200 °C
 230 MPa
@Strain 0.2 %,
Temperature 200 °C
 235 MPa
@Strain 0.2 %,
Temperature 150 °C
 235 MPa
@Strain 0.2 %,
Temperature 150 °C
 >= 240 MPa
@Strain 0.2 %,
Temperature 100 °C
Elongation at Break >= 20 %
@Diameter <=3.00 mm
 >= 20 %
@Diameter >=3.00 mm
Modulus of Elasticity 220 GPa
 200 GPa
@Temperature 400 °C
 205 GPa
@Temperature 300 °C
 210 GPa
@Temperature 200 °C
 215 GPa
@Temperature 100 °C
Charpy Impact, Notched >= 100 J/cm²
 
Thermal PropertiesOriginal ValueComments
CTE, linear 10.5 µm/m-°C
@Temperature 20.0 - 100 °C
 11.0 µm/m-°C
@Temperature 20.0 - 200 °C
 11.5 µm/m-°C
@Temperature 20.0 - 300 °C
 12.0 µm/m-°C
@Temperature 20.0 - 400 °C
 12.5 µm/m-°C
@Temperature 20.0 - 500 °C
Specific Heat Capacity 0.460 J/g-°C
@Temperature 20.0 °C
Thermal Conductivity 25.0 W/m-K
@Temperature 20.0 °C
 
Component Elements PropertiesOriginal ValueComments
Carbon, C <= 0.030 %
Chromium, Cr 10.5 - 12.5 %
Iron, Fe 82.4 - 86.7 %As Balance
Manganese, Mn 1.5 %
Nickel, Ni 0.30 - 1.0 %
Nitrogen, N 0.030 %
Phosphorus, P <= 0.040 %
Silicon, Si 1.0 - 2.5 %
Sulfur, S <= 0.015 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
304 Stainless Steel
409 Stainless Steel
AISI 15B62H Carbon Steel, Composition Spec
Covestro Bayblend® R-T 60 Polycarbonate/ABS Blend
Sandvik 5CR12 Ti Plate, Sheet and Coil

NSANDV201 / 19095

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.