MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Hexcel® HexBond™ ST1480.06 NW 292g/m2 Epoxy Film Adhesive
Categories: Polymer; Thermoset; Epoxy; Epoxy Adhesive

Material Notes: Description: HexBond™ ST1480 is a modified epoxy film adhesive. This 180°C/356°F cure film adhesive is specially designed for bonding metal-to-metal and composite-to-composite structures. Its formulation, based on epoxy resin, provides high peel strength and toughness with high sheer strength.

Features:

  • Excellent metal-to-metal peel strength and composite-to-composite bonding
  • 180°C/356°F cure
  • Service temperature from -55°C to 150°C (-67°F to 302°F)
  • Excellent moisture resistance in high humidity environments
  • Available in a wide range of film thicknesses
Applications:
  • Metal-to-metal bonding
  • Sandwich construction
  • Composite-to-composite bonding

Information provided by Hexcel Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesMetricEnglishComments
Adhesive Bond Strength  18.6 MPa
@Temperature 80.0 °C
2700 psi
@Temperature 176 °F
Single Lap Shear Strength Metal/Metal, 2000 hours 70°C in hydraulic fluid; EN 2243-1
 21.8 MPa
@Temperature 80.0 °C
3160 psi
@Temperature 176 °F
Single Lap Shear Strength Composite/Composite, 2000 hours 70°C / 158°F 85% RH, Cure 2; AITM 1-0019
 23.1 MPa
@Temperature 150 °C
3350 psi
@Temperature 302 °F
Single Lap Shear Strength Metal/Metal; EN 2243-1
 23.5 MPa
@Temperature 80.0 °C
3410 psi
@Temperature 176 °F
Single Lap Shear Strength Metal/Metal, 2000 hours 50°C in hydraulic fluid/water mixture; EN 2243-1
 24.4 MPa
@Temperature 275 °C
3540 psi
@Temperature 527 °F
Single Lap Shear Strength Composite/Composite; AITM 1-0019
 25.6 MPa
@Temperature 80.0 °C
3710 psi
@Temperature 176 °F
Single Lap Shear Strength Metal/Metal, 24 hours 23°C in solvent; EN 2243-1
 25.8 MPa
@Temperature 120 °C
3740 psi
@Temperature 248 °F
Single Lap Shear Strength Metal/Metal; EN 2243-1
 25.9 MPa
@Temperature 22.8 °C
3760 psi
@Temperature 73.0 °F
Single Lap Shear Strength Metal/Metal, 2000 hours 70°C in hydraulic fluid; EN 2243-1
 27.0 MPa
@Temperature 80.0 °C
3920 psi
@Temperature 176 °F
Single Lap Shear Strength Metal/Metal; EN 2243-1
 28.2 MPa
@Temperature 22.8 °C
4090 psi
@Temperature 73.0 °F
Single Lap Shear Strength Metal/Metal, 2000 hours 50°C in hydraulic fluid/water mixture; EN 2243-1
 28.2 MPa
@Temperature 22.8 °C
4090 psi
@Temperature 73.0 °F
Single Lap Shear Strength Metal/Metal, 24 hours 23°C in solvent; EN 2243-1
 28.5 MPa
@Temperature 22.8 °C
4130 psi
@Temperature 73.0 °F
Single Lap Shear Strength Metal/Metal; EN 2243-1
 29.3 MPa
@Temperature -55.0 °C
4250 psi
@Temperature -67.0 °F
Single Lap Shear Strength Metal/Metal; EN 2243-1
 29.9 MPa
@Temperature 22.8 °C
4340 psi
@Temperature 73.0 °F
Single Lap Shear Strength Composite/Composite, 2000 hours 70°C / 158°F 85% RH, Cure 1; AITM 1-0019
 30.1 MPa
@Temperature 80.0 °C
4370 psi
@Temperature 176 °F
Single Lap Shear Strength Composite/Composite; AITM 1-0019
 32.6 MPa
@Temperature 22.8 °C
4730 psi
@Temperature 73.0 °F
Single Lap Shear Strength Composite/Composite; AITM 1-0019
 
Thermal PropertiesMetricEnglishComments
Glass Transition Temp, Tg 111 °C232 °F4h at 150°C, 2000 hours 70°C / 158°F
 119 °C246 °F90 min at 180°C, 2000 hours 70°C / 158°F 85% RH
 180 °C356 °F4h at 150°C
 193 °C379 °F90 min at 180°C
 
Processing PropertiesMetricEnglishComments
Cure Time 90.0 min
@Temperature 180 °C
1.50 hour
@Temperature 356 °F
 
Descriptive Properties
Climbing drum peel torque113 N/25mm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PHEXCB9275 / 322431

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.