MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Chemours Viton® GBL-600S with 8650, 1 phr, Car. Wax Fluoroelastomer Compound
Categories: Polymer; Thermoset; Fluoropolymer, TS; Thermoset Fluoroelastomer; Rubber or Thermoset Elastomer (TSE)

Material Notes:
  • Cures exceptionally fast to a high state of cure
  • Exhibits improved mold release/mold fouling properties compared to Viton® GBL-900 and Viton® GBL-200
  • Exhibits improved mold flow, less shear sensitivity, and lower extruder die swell for a 65 Mooney FKM
  • Exhibits excellent physical properties with high elongation, both original and aged
  • Exhibits similar heat, fluids, and low temperature resistance compared to Viton® GBL-900 and Viton® GBL-200
  • Exhibits excellent compression set resistance with short (2 hr) or no postcure

Chemours was formed from former DuPont performance chemicals businesses, including the Viton product line, in 2015.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 70No Postcure; ASTM D2240
 732 hours Postcure; ASTM D2240
 745.5 hours Postcure; ASTM D2240
 758 hours Postcure; ASTM D2240
Tensile Strength at Break 10.5 MPaNo Postcure; ASTM D412
 12.3 MPa2 hours Postcure; ASTM D412
 16.7 MPa5.5 hours Postcure; ASTM D412
 18.4 MPa8 hours Postcure; ASTM D412
Tensile Stress at Strain 0.900 MPa
@Strain 10 %
No Postcure; ASTM D412
 1.00 MPa
@Strain 10 %
2 hours Postcure; ASTM D412
 1.00 MPa
@Strain 10 %
5.5 hours Postcure; ASTM D412
 1.10 MPa
@Strain 10 %
8 hours Postcure; ASTM D412
Elongation at Break 336 %5.5 hours Postcure; ASTM D412
 339 %8 hours Postcure; ASTM D412
 361 %2 hours Postcure; ASTM D412
 380 %No Postcure; ASTM D412
100% Modulus 0.00290 GPa
@Strain 100 %
No Postcure; ASTM D412
 0.00340 GPa
@Strain 100 %
2 hours Postcure; ASTM D412
 0.00380 GPa
@Strain 100 %
5.5 hours Postcure; ASTM D412
 0.00400 GPa
@Strain 100 %
8 hours Postcure; ASTM D412
Compression Set 13 %
@Temperature 200 °C,
Time 79200 sec
Plied Discs, 5.5 hours postcured; ASTM D395B
 14 %
@Temperature 200 °C,
Time 79200 sec
Plied Discs, 8 hours postcured; ASTM D395B
 14 %
@Temperature 200 °C,
Time 79200 sec
Plied Discs, postcured 2hrs; ASTM D395B
 14 %
@Temperature 200 °C,
Time 79200 sec
O-Rings, 8 hours postcured; ASTM D395B
 17 %
@Temperature 200 °C,
Time 252000 sec
Plied Discs, 5.5 hours postcured; ASTM D395B
 18 %
@Temperature 200 °C,
Time 252000 sec
Plied Discs, 8 hours postcured; ASTM D395B
 19 %
@Temperature 200 °C,
Time 79200 sec
O-Rings, 5.5 hours postcured; ASTM D395B
 20 %
@Temperature 200 °C,
Time 79200 sec
O-Rings, postcured 2hrs; ASTM D395B
 20 %
@Temperature 200 °C,
Time 252000 sec
Plied Discs, postcured 2hrs; ASTM D395B
 21 %
@Temperature 200 °C,
Time 252000 sec
O-Rings, 5.5 hours postcured; ASTM D395B
 23 %
@Temperature 200 °C,
Time 252000 sec
O-Rings, 8 hours postcured; ASTM D395B
 27 %
@Temperature 200 °C,
Time 79200 sec
O-Rings, no postcure; ASTM D395B
 33 %
@Temperature 200 °C,
Time 252000 sec
O-Rings, postcured 2hrs; ASTM D395B
 43 %
@Temperature 200 °C,
Time 252000 sec
O-Rings, Cured 70hrs, no postcure; ASTM D395B
 
Thermal PropertiesOriginal ValueComments
Glass Transition Temp, Tg -21.2 °CNo Postcure
 -18.6 °C2 hours Postcure
 -18.2 °C5.5 hours Postcure
 -18.0 °C8 hours Postcure
 
Processing PropertiesOriginal ValueComments
Processing Temperature 177 °C
@Time 421 sec
Cure
 232 °C
@Time 7200 - 28800 sec
Postcure
 
Component Elements PropertiesOriginal ValueComments
Fluorine, F 68 %Uncompounded Viton
 
Descriptive Properties
Compound NumberA26-04
Formulation as Tested1Carnauba Wax
 100GBL-600S
 2Varox® DBPH-50
 3Zinc Oxide
 3Diak 7 (TAIC)
 30MT Black

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Dow 2-5088 Wax
Chemours Viton® GBL-600S with 8650, 0.5 phr, WS280 Fluoroelastomer Compound
Chemours Viton® GBL-600S with 8650, 0.5 phr, 8D Fluoroelastomer Compound
Chemours Viton® GBL-600S with 60-MT Black Fluoroelastomer Compound
Chemours Viton® GBL-600S with 5-MT Black Fluoroelastomer Compound

PDVC9824 / 170465

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.