MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Extreme Materials from MCAM
Visit Mitsubishi Chemical Advanced Materials for Extreme Materials - high performance plastic machining stock engineered to replace metals such as nickel alloys or stainless steel.

(Viewing data as-entered. Click here to return)
AFE Technologies Cronite Standard Nickel Alloy Castings, No. HR4
Categories: Metal; Nonferrous Metal; Nickel Alloy; Superalloy

Material Notes: High temperature nickel alloy castings. Applications include heat treatment and handling products, furnace products, tubes, power generation, and petrochemical industries.

Information provided by AFE Technologies/North American Cronite, Inc.


Composition Notes: Tungsten added but not quantified in composition table.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 500 MPaAs Cast
Tensile Strength, Yield 260 MPaAs Cast
Elongation at Break 8.0 %As Cast; 5.65 A0.5
Rupture Strength 3.80 MPa
@Temperature 1150 °C,
Time 3.60e+7 sec
Stress Rupture
 6.00 MPa
@Temperature 1100 °C,
Time 3.60e+7 sec
Stress Rupture
 9.30 MPa
@Temperature 1050 °C,
Time 3.60e+7 sec
Stress Rupture
 14.0 MPa
@Temperature 1000 °C,
Time 3.60e+7 sec
Stress Rupture
 20.0 MPa
@Temperature 950 °C,
Time 3.60e+7 sec
Stress Rupture
 28.0 MPa
@Temperature 900 °C,
Time 3.60e+7 sec
Stress Rupture
 39.0 MPa
@Temperature 850 °C,
Time 3.60e+7 sec
Stress Rupture
 52.0 MPa
@Temperature 800 °C,
Time 3.60e+7 sec
Stress Rupture
 70.0 MPa
@Temperature 750 °C,
Time 3.60e+7 sec
Stress Rupture
 93.0 MPa
@Temperature 700 °C,
Time 3.60e+7 sec
Stress Rupture
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.50 %
Chromium, Cr 18 %
Iron, Fe 27 %As Remainder
Manganese, Mn 1.0 %
Nickel, Ni 52 %
Silicon, Si 1.5 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Special Metals NIMONIC® Alloy 115
MV Labs CR800 Cr2O3 Chromium(III) oxide
H.C. Starck Amperit® 705.1 Fused Chromium Oxide 96.0 % (Cr2O3)
H.C. Starck Amperit® 703.053 Chromium Oxide (Cr2O3) 99.5%
Chromium (III) Oxide, Cr2O3 (Eskolaite)

NCRON04 / 15989

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.