MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

CRP  Windform

(Viewing data as-entered. Click here to return)
Huntsman Iroprint™ F 53177 Polyester-Based TPU Protoyping Filament
Categories: Polymer; 3D Printing/Additive Manufacturing Polymer; Thermoplastic; Polyurethane, TP; Thermoplastic Polyurethane, Elastomer, Polyester Grade

Material Notes: IROPRINT F 53117 is a polyester-based Thermoplastic Polyurethane (TPU) for Fused Filament Fabrication (FFF). Key features are high elasticity, abrasion resistance, cut and scratch resistance and good low temperature performance. IROPRINT F53117 is an all-round grade, easy to print and with high mechanical properties.

Applications: Footwear, hoses and gaskets, robotic grippers, seals and other applications that need to be soft and elastic, yet strong and tough.

Information provided by Huntsman.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 1.221 g/ccISO 1183-1
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 96
@Time 3.00 sec
ISO 7619
Hardness, Shore D 51
@Time 3.00 sec
ISO 7619
Tensile Strength 24.0 MPaZ Orientation; DIN 53504
 43.0 MPaXY Orientation; DIN 53504
Elongation at Break 270 %Z Orientation; DIN 53504
 480 %XY Orientation; DIN 53504
Tear Strength 80.0 kN/mZ Orientation; ISO 34-1
 175 kN/mXY Orientation; ISO 34-1
Abrasion 35mm3; XY Orientation; ISO 4649
Compression Set 30 %
@Temperature 23.0 °C,
Time 252000 sec
XY Orientation; ASTM D395
 
Processing PropertiesOriginal ValueComments
Nozzle Temperature 250 °C
 
Descriptive Properties
Bed Temperature20-80°C
Extrusion Multiplier (Flow)1.8
Fan Speed100%
Nozzle Diameter0.4 mm
Print Speed10-100 mm/s

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PHU9880 / 255828

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.