MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Chang Chun Plastic PBT3015 15% Glass Fiber Enforced PBT
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), 20% Glass Fiber Filled

Material Notes: Information provided by Dowell Trading Company Ltd.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.39 - 1.43 g/ccASTM D792
Water Absorption 0.040 %24 hour immersion; ASTM D570
Linear Mold Shrinkage 0.0040 - 0.020 cm/cmASTM D955
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 93ASTM D785
Tensile Strength, Ultimate 80.0 - 100 MPaASTM D638
Elongation at Break 4.0 - 5.0 %ASTM D638
Flexural Yield Strength 130 - 150 MPaASTM D790
Flexural Modulus 4.00 - 5.00 GPaASTM D790
Izod Impact, Notched 0.500 - 0.700 J/cm
@Thickness 6.35 mm
ASTM D256
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity >= 1.00e+16 ohm-cmASTM D257
Surface Resistance >= 1.00e+14 ohmASTM D257
Dielectric Constant 3.3
@Frequency 60 Hz
ASTM D150
Dielectric Strength 20.0 kV/mm
@Thickness 2.00 mm
ASTM D149
Dissipation Factor 0.0010
@Frequency 60 Hz
ASTM D150
Arc Resistance 129 secASTM D495
 
Thermal PropertiesOriginal ValueComments
CTE, linear 50.0 µm/m-°C
@Temperature 20.0 °C
ASTM D696
Melting Point 225 °CDSC
Deflection Temperature at 0.46 MPa (66 psi) 220 °CASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 206 °CASTM D648
Flammability, UL94 HB
@Thickness 0.7937 mm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Chang Chun Plastic PBT3030 30% Glass Fiber Enforced PBT
Overview of materials for Polybutylene Terephthalate (PBT), 20% Glass Fiber Filled
Gromax PBT 1100-211M
Gromax PBT 3020-104 15% Glass Fiber Filled
Chang Chun Plastic PBT2100 Fire Retardant PBT

PDOWELC34 / 30765

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.