MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger SPI

SABIC ULTEM™ Resin 1010 Polyetherimide (PEI)
Categories: Polymer; Thermoplastic; Polyetherimide (PEI)

Material Notes: ULTEM 1010 Resin is an unreinforced amorphous polyetherimide (PEI) resin that may offer a high glass transition temperature (Tg) of 217°C and improved flow. Features are excellent mechanical, electrical and dimensional properties up to high temperatures. The material may offer very good chemical resistance for an amorphous material and is inherently flame retardant offering UL94 V0 and 5V ratings and aerospace FAR 25.853 compliance. The material is RoHS compliant and the natural, uncolored, material is halogen free according to standards IEC 61249-2-21, IPC 4101E and JEDEC JS709B. For colored variants compliance needs to be checked case by case. The base material is transparent amber colored but is also available in custom colors - transparent and opaque.

Features: Transparent to Microwave radiation and near IR,Metallizable,Radiation Resistance (gamma, x-ray),UV-C Resistance,High electric breakdown strength (BDS),High Stiffness,Hydrolytic Stability,Chemical Resistance,Easy Flow,Low Smoke and Toxicity,Good Mechanicals in Broad Temperature Range,Low Creep Sensitivity,Low Shrinkage,Good metal adhesion,Amorphous,High Strength,General Purpose,High Heat Resistance,Good dimensional stability,Flame Retardant,Transparent

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.27 g/cc1.27 g/ccASTM D792
Density 1.27 g/cc0.0459 lb/in³ISO 1183
Water Absorption  0.25 %
@Time 86400 sec
0.25 %
@Time 24.0 hour
ASTM D570
 0.25 %
@Time 86400 sec
0.25 %
@Time 24.0 hour
ISO 62-1
Moisture Absorption 0.0100 - 0.0200 %0.0100 - 0.0200 %Extrusion Blow Molding
 0.0200 %0.0200 %Injection Molding
 0.200 %0.200 %23°C/50% RH/24 hrs; ISO 62-4
Moisture Absorption at Equilibrium 0.70 %0.70 %23°C/50% RH; ISO 62-4
Water Absorption at Saturation 1.25 %1.25 %ASTM D570
 1.25 %1.25 %ISO 62-1
Viscosity  13 cP
@Load 5.00 kg,
Temperature 340 °C
13 cP
@Load 11.0 lb,
Temperature 644 °F
MVR cc/10 min; ISO 1133
 25 cP
@Load 5.00 kg,
Temperature 360 °C
25 cP
@Load 11.0 lb,
Temperature 680 °F
MVR cc/10 min; ISO 1133
Linear Mold Shrinkage, Flow 0.0050 - 0.0070 cm/cm
@Thickness 3.20 mm
0.0050 - 0.0070 in/in
@Thickness 0.126 in
SABIC method
Linear Mold Shrinkage, Transverse 0.0050 - 0.0070 cm/cm
@Thickness 3.20 mm
0.0050 - 0.0070 in/in
@Thickness 0.126 in
SABIC method
Melt Flow 17.8 g/10 min
@Load 6.60 kg,
Temperature 337 °C
17.8 g/10 min
@Load 14.6 lb,
Temperature 639 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 106106ISO 2039-2
 109109ASTM D785
Ball Indentation Hardness 140 MPa20300 psiH358/30; ISO 2039-1
Tensile Strength, Yield 110 MPa16000 psi5 mm/min; ASTM D638
 110 MPa16000 psi50 mm/min; ISO 527
 115 MPa16700 psi50 mm/min; ASTM D638
Elongation at Break 50 %50 %50 mm/min; ISO 527
 60 %60 %5 mm/min; ASTM D638
 60 %60 %50 mm/min; ASTM D638
Elongation at Yield 6.0 %6.0 %50 mm/min; ISO 527
 7.0 %7.0 %5 mm/min; ASTM D638
 7.0 %7.0 %50 mm/min; ASTM D638
Tensile Modulus 3.20 GPa464 ksi1 mm/min; ISO 527
 3.35 GPa486 ksi5 mm/min; ASTM D638
Flexural Strength 160 MPa23200 psiyld, 2.6 mm/min, 100 mm span; ASTM D790
 160 MPa23200 psiyield, 2 mm/min; ISO 178
 165 MPa23900 psiyld, 1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 3.20 GPa464 ksi1.3 mm/min, 50 mm span; ASTM D790
 3.30 GPa479 ksi2 mm/min; ISO 178
 3.40 GPa493 ksi2.6 mm/min, 100 mm span; ASTM D790
Poissons Ratio 0.360.36ASTM E132
Izod Impact Notched 32.0 J23.6 ft-lbASTM D256
 41.0 J
@Temperature -30.0 °C
30.2 ft-lb
@Temperature -22.0 °F
ASTM D256
 1174 J
@Thickness 3.20 mm
865.9 ft-lb
@Thickness 0.126 in
reverse notched; ASTM D256
Izod Impact, Unnotched 16.0 J/cm30.0 ft-lb/inASTM D4812
 15.0 J/cm
@Temperature -30.0 °C
28.1 ft-lb/in
@Temperature -22.0 °F
ASTM D4812
Izod Impact, Notched (ISO) 5.00 kJ/m²2.38 ft-lb/in²80*10*4; ISO 180/1A
 5.00 kJ/m²
@Temperature -30.0 °C
2.38 ft-lb/in²
@Temperature -22.0 °F
80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) NBNB80*10*4; ISO 180/1U
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
80*10*4; ISO 180/1U
Charpy Impact, Notched 0.400 J/cm²1.90 ft-lb/in²Edgew 80*10*4 sp=62mm; ISO 179/1eA
 0.400 J/cm²
@Temperature -30.0 °C
1.90 ft-lb/in²
@Temperature -22.0 °F
Edgew 80*10*4 sp=62mm; ISO 179/1eA
Gardner Impact 33.0 J24.3 ft-lbSABIC method
Taber Abrasion, mg/1000 Cycles 1010CS-17, 1 kg; ASTM D1044
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+15 ohm-cm1.00e+15 ohm-cmIEC 60093
 1.00e+17 ohm-cm1.00e+17 ohm-cmASTM D257
Surface Resistance >= 1.00e+15 ohm>= 1.00e+15 ohmROA; IEC 60093
Dielectric Constant  2.9
@Frequency 1e+6 Hz
2.9
@Frequency 1e+6 Hz
IEC 60250
 2.9
@Frequency 50.0 - 60.0 Hz
2.9
@Frequency 50.0 - 60.0 Hz
IEC 60250
 3.01
@Frequency 1.10e+9 Hz
3.01
@Frequency 1.10e+9 Hz
 3.02
@Frequency 5.00e+9 Hz
3.02
@Frequency 5.00e+9 Hz
 3.02
@Frequency 1e+10 Hz
3.02
@Frequency 1e+10 Hz
 3.15
@Frequency 1000 Hz
3.15
@Frequency 1000 Hz
ASTM D150
 3.15
@Frequency 100 Hz
3.15
@Frequency 100 Hz
ASTM D150
Dielectric Strength  16.0 kV/mm
@Thickness 3.20 mm
406 kV/in
@Thickness 0.126 in
in oil; IEC 60243-1
 19.7 kV/mm
@Thickness 3.20 mm
500 kV/in
@Thickness 0.126 in
in oil; ASTM D149
 25.0 kV/mm
@Thickness 1.60 mm
635 kV/in
@Thickness 0.0630 in
in oil; IEC 60243-1
 28.0 kV/mm
@Thickness 1.60 mm
711 kV/in
@Thickness 0.0630 in
in oil; ASTM D149
 32.7 kV/mm
@Thickness 1.60 mm
831 kV/in
@Thickness 0.0630 in
in air; ASTM D149
 33.0 kV/mm
@Thickness 0.800 mm
838 kV/in
@Thickness 0.0315 in
in oil; IEC 60243-1
Dissipation Factor  0.00050
@Frequency 50.0 - 60.0 Hz
0.00050
@Frequency 50.0 - 60.0 Hz
IEC 60250
 0.0012
@Frequency 1000 Hz
0.0012
@Frequency 1000 Hz
ASTM D150
 0.0012
@Frequency 1.10e+9 Hz
0.0012
@Frequency 1.10e+9 Hz
 0.0015
@Frequency 100 Hz
0.0015
@Frequency 100 Hz
ASTM D150
 0.0024
@Frequency 5.00e+9 Hz
0.0024
@Frequency 5.00e+9 Hz
 0.0027
@Frequency 1e+10 Hz
0.0027
@Frequency 1e+10 Hz
 0.0060
@Frequency 1e+6 Hz
0.0060
@Frequency 1e+6 Hz
IEC 60250
Arc Resistance 120 - 180 sec120 - 180 secASTM D495
Comparative Tracking Index 100 V100 VIEC 60112
 100 - 175 V100 - 175 VUL 746A
 150 V150 VIEC 60112
Hot Wire Ignition, HWI  30 - 60 sec
@Thickness >=0.750 mm
30 - 60 sec
@Thickness >=0.0295 in
UL 746A
 60 - 120 sec
@Thickness >=3.00 mm
60 - 120 sec
@Thickness >=0.118 in
UL 746A
High Amp Arc Ignition, HAI  0.00 - 15 arcs
@Thickness >=0.750 mm
0.00 - 15 arcs
@Thickness >=0.0295 in
UL 746A
 15 - 30 arcs
@Thickness >=3.00 mm
15 - 30 arcs
@Thickness >=0.118 in
UL 746A
High Voltage Arc-Tracking Rate, HVTR 25.4 - 80.0 mm/min1.00 - 3.15 in/minUL 746A
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow  52.0 µm/m-°C
@Temperature -20.0 - 150 °C
28.9 µin/in-°F
@Temperature -4.00 - 302 °F
ISO 11359-2
 56.0 µm/m-°C
@Temperature -20.0 - 150 °C
31.1 µin/in-°F
@Temperature -4.00 - 302 °F
ASTM E831
CTE, linear, Transverse to Flow  52.0 µm/m-°C
@Temperature -20.0 - 150 °C
28.9 µin/in-°F
@Temperature -4.00 - 302 °F
ISO 11359-2
 54.0 µm/m-°C
@Temperature -20.0 - 150 °C
30.0 µin/in-°F
@Temperature -4.00 - 302 °F
ASTM E831
Thermal Conductivity 0.220 W/m-K1.53 BTU-in/hr-ft²-°FASTM C177
 0.220 W/m-K1.53 BTU-in/hr-ft²-°FISO 8302
Hot Ball Pressure Test 125 °C257 °FPASS; IEC 60695-10-2
Deflection Temperature at 0.46 MPa (66 psi) 209 °C408 °FFlatw 80*10*4 sp=64mm; ISO 75/Bf
 207 °C
@Thickness 3.20 mm
405 °F
@Thickness 0.126 in
unannealed; ASTM D648
 210 °C
@Thickness 6.40 mm
410 °F
@Thickness 0.252 in
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 192 °C378 °FFlatw 80*10*4 sp=64mm; ISO 75/Af
 190 °C
@Thickness 3.20 mm
374 °F
@Thickness 0.126 in
unannealed; ASTM D648
 201 °C
@Thickness 6.40 mm
394 °F
@Thickness 0.252 in
unannealed; ASTM D648
Vicat Softening Point 211 °C412 °FRate B/50; ASTM D1525
 211 °C412 °FRate B/50; ISO 306
 212 °C414 °FRate B/120; ISO 306
 215 °C419 °FRate A/50; ISO 306
UL RTI, Electrical 170 °C338 °FUL 746B
UL RTI, Mechanical with Impact 170 °C338 °FUL 746B
UL RTI, Mechanical without Impact 170 °C338 °FUL 746B
Flammability, UL94  V-2
@Thickness >=0.400 mm
V-2
@Thickness >=0.0157 in
UL 94
 V-0
@Thickness >=0.750 mm
V-0
@Thickness >=0.0295 in
UL 94
 5VA
@Thickness >=3.00 mm
5VA
@Thickness >=0.118 in
UL 94
Smoke Density 2.02.0Flaming, Ds 4 min; ASTM E662
Oxygen Index 44 %44 %ASTM D2863
 47 %47 %ISO 4589
Glow Wire Flammability Index 960 °C
@Thickness 3.20 mm
1760 °F
@Thickness 0.126 in
IEC 60695-2-12
 
Processing PropertiesMetricEnglishComments
Nozzle Temperature 345 - 405 °C653 - 761 °F
Zone 1 325 - 350 °C617 - 662 °FExtrusion Blow Molding
Zone 2 330 - 355 °C626 - 671 °FExtrusion Blow Molding
 340 - 405 °C644 - 761 °F
Zone 3 330 - 355 °C626 - 671 °FExtrusion Blow Molding
 345 - 415 °C653 - 779 °F
Zone 4 330 - 355 °C626 - 671 °FExtrusion Blow Molding
Zone 5 330 - 355 °C626 - 671 °F
Die Temperature 325 - 355 °C617 - 671 °FExtrusion Blow Molding
Melt Temperature 320 - 355 °C608 - 671 °FExtrusion Blow Molding
 350 - 410 °C662 - 770 °FInjection Molding
Head Temperature 330 - 355 °C626 - 671 °FZone 6 - Top Temperature
 330 - 355 °C626 - 671 °FZone 7 - Bottom Temperature
Mold Temperature 65.0 - 175 °C149 - 347 °F
 135 - 180 °C275 - 356 °F
Drying Temperature 140 - 150 °C284 - 302 °FExtrusion Blow Molding
 150 °C302 °FInjection Molding
Dry Time 4.00 - 6.00 hour4.00 - 6.00 hourInjection Molding
 4.00 - 6.00 hour4.00 - 6.00 hourExtrusion Blow Molding
 24.0 hour24.0 hourCumulative; Injection Molding
 24.0 hour24.0 hourCumulative; Extrusion Blow Molding
Back Pressure 0.300 - 0.700 MPa43.5 - 102 psi
Shot Size 40 - 60 %40 - 60 %
Vent Depth 0.00250 - 0.00760 cm0.000984 - 0.00299 in
Screw Speed 10 - 70 rpm10 - 70 rpm
 
Descriptive Properties
Screw speed (Circumferential speed)0.2-0.3 m/s

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABH82504 / 290451

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.