MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
EMS-Grivory Grilon® TSS/4 LF 1 PA666
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6/66

Material Notes: Product description: Grilon TSS/4 LF 1 is a heat stabilized, normal viscosity PA66 + PA6 injection molding grade with 1% lubricant (molybdenum disulphide). Grilon TSS/4 LF 1 has the following important properties:
  • Low sliding friction
  • High surface hardness
  • Short cycle times
Grilon TSS/4 LF 1 is typically used for oil dip sticks, low stressed slide rings, and damping elements.

Information provided by EMS Grivory.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.15 g/ccDry; ISO 1183
Water Absorption 5.0 %Sim. to ISO 62
Moisture Absorption 2.00 %Sim. to ISO 62
Linear Mold Shrinkage, Flow 0.0090 cm/cmISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.010 cm/cmISO 294-4, 2577
 
Mechanical PropertiesOriginal ValueComments
Ball Indentation Hardness 65.0 MPaConditioned; ISO 2039-1
 140 MPaDry; ISO 2039-1
Tensile Strength at Break 70.0 MPaDry; ISO 527-1/-2
Tensile Strength, Yield 50.0 MPaConditioned; ISO 527-1/-2
 90.0 MPaDry; ISO 527-1/-2
Elongation at Break 12 %Nominal, Dry; ISO 527-1/-2
 >= 50 %Nominal, Conditioned; ISO 527-1/-2
Elongation at Yield 5.0 %Dry; ISO 527-1/-2
 15 %Conditioned; ISO 527-1/-2
Tensile Modulus 1400 MPaConditioned; ISO 527-1/-2
 3300 MPaDry; ISO 527-1/-2
Charpy Impact Unnotched NB
@Temperature 23.0 °C
Conditioned; ISO 179/1eU
 NB
@Temperature -30.0 °C
Conditioned; ISO 179/1eU
 NB
@Temperature 23.0 °C
Dry; ISO 179/1eU
 NB
@Temperature -30.0 °C
Dry; ISO 179/1eU
Charpy Impact, Notched 4.00 kJ/m²
@Temperature -30.0 °C
Dry; ISO 179/1eA
 4.00 kJ/m²
@Temperature 23.0 °C
Dry; ISO 179/1eA
 4.00 kJ/m²
@Temperature -30.0 °C
Conditioned; ISO 179/1eA
 8.00 kJ/m²
@Temperature 23.0 °C
Conditioned; ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+10 ohm-cmConditioned; IEC 60093
 1.00e+12 ohm-cmDry; IEC 60093
Surface Resistance 1.00e+11 ohmIEC 60093
Dielectric Strength 25.0 kV/mmConditioned; IEC 60243-1
 27.0 kV/mmDry; IEC 60243-1
Comparative Tracking Index 475 VConditioned; IEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 80.0 µm/m-°CISO 11359-1/-2
CTE, linear, Transverse to Flow 90.0 µm/m-°CISO 11359-1/-2
Melting Point 260 °C10°C/min; ISO 11357-1/-3
Maximum Service Temperature, Air 80.0 - 100 °CLong Term; ISO 2578
 220 °CShort Term; EMS
Deflection Temperature at 1.8 MPa (264 psi) 85.0 °CISO 75-1/-2
Deflection Temperature at 8.0 MPa 65.0 °CISO 75-1/-2
Flammability, UL94 HBIEC 60695-11-10
 
Descriptive Properties
AutomotiveInterior
 Powertrain and Chassis
FormGranules
Industry & Consumer goodsMechanical Engineering
 Power transmission
 Tools & Accessories
ProcessingInjection Molding
Product AttributesImproved friction & wear properties

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Kuraray HYBRAR® Low Rebound Compound # 1
Ensinger Tecast Vekton™ 6XAU High Heat Cast Nylon 6 (PA6)
Ensinger Tecast Vekton™ 6PAM MoS2-Filled Cast Nylon 6 (PA6)
Dow BETAPHON™ 2 Synthetic Rubber
Dow BETADAMP™ 24 Vibration Damper

PGRH303 / 157012

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.