MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
CRP Technology PA12 SLS Black Nylon 12 for SLS 3D Printing
Categories: Polymer; 3D Printing/Additive Manufacturing Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 12 (PA12)

Material Notes: Good mechanical properties, low density, resistant to abrasion, water, and solvents.

Distinguished for its dark black color, PA12 SLS Black is a versatile cost-effective ally for a wide range of industrial applications in many sectors:- connectors, hinges, housings and enclosures, jigs and fixtures just to cite a few. By PA12 SLS Black allows complex geometries and thin walls even for small objects, including functional prototypes, small series, and limited editions.

Information provided by CRP Technology.

Key Words: Selective Laser Sintering
Vendors:   About CRP Technology
CRP Technology (Modena, Italy) develops, manufactures and sells its proprietary high performance composite materials Windform® for professional 3D Printing. It is also distinguished by its know-how in Selective Laser Sintering technology. It offers part production for short- and low-run production, and prototyping services with Windform®. Its specific application fields including but are not limited to: automotive and motorsports, design, aerospace, UAVs, marine, entertainment, defense, and packaging.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 0.990 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 78UNI EN ISO 868
Tensile Strength at Break 45.78 MPaZX Axis; UNI EN ISO 527-1
 47.84 MPaXY Axis; UNI EN ISO 527-1
 47.92 MPaYX Axis; UNI EN ISO 527-1
Elongation at Break 8.7 %ZX Axis; UNI EN ISO 527-1
 11.06 %YX Axis; UNI EN ISO 527-1
 12.18 %XY Axis; UNI EN ISO 527-1
Tensile Modulus 1.868 GPaZX Axis; UNI EN ISO 527-1
 1.907 GPaXY Axis; UNI EN ISO 527-1
 1.919 GPaYX Axis; UNI EN ISO 527-1
Flexural Strength 68.84 MPaUNI EN ISO 14125
Flexural Modulus 1.628 GPaUNI EN ISO 14125
Izod Impact, Notched (ISO) 4.70 kJ/m²
@Temperature -40.0 °C
UNI EN ISO 180
 4.90 kJ/m²
@Temperature 23.0 °C
UNI EN ISO 180
Izod Impact, Unnotched (ISO) 18.5 kJ/m²
@Temperature -40.0 °C
UNI EN ISO 180
 19.9 kJ/m²
@Temperature 23.0 °C
UNI EN ISO 180
Charpy Impact Unnotched 2.26 J/cm²
@Temperature -30.0 °C
UNI EN ISO 179-1
 2.54 J/cm²
@Temperature 23.0 °C
UNI EN ISO 179-1
Charpy Impact, Notched 0.400 J/cm²
@Temperature -30.0 °C
UNI EN ISO 179-1
 0.430 J/cm²
@Temperature 23.0 °C
UNI EN ISO 179-1
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.5e+14 ohm-cmASTM D257-14
Surface Resistance 9.3e+14 ohmASTM D257-14
Comparative Tracking Index 600 VIEC 60112 Solution A
 
Thermal PropertiesOriginal ValueComments
Melting Point 181.7 °CISO 11357
 
Descriptive Properties
ColorDark Black
Specific Flexural Modulus1643 MPa/(g/cc)Flexural Modulus per density unit
Specific Flexural Strength69.47 MPa/(g/cc)Flexural Strength per density unit
Specific Tensile Modulus1925 MPa/(g/cc)Tensile Modulus per density unit
Specific Tensile Strength48.27 MPa/(g/cc)UTS per density unit
Surface Finish0.42 Ra µmAfter CNC machining
 1.83 Ra µmAfter Manual Finishing
 8.17 Ra µmAfter SLS Process

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PCRPT40x / 318860

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.