MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Polykemi AB POLYabs H00 HF ABS, Heat Resistant, High Flow
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylonitrile Butadiene Styrene (ABS), Heat Resistant, Molded

Material Notes:

Information provided by Polykemi AB

Key Words: ABS
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.05 g/cc0.0379 lb/in³ISO 1183
Linear Mold Shrinkage, Flow 0.0060 - 0.0080 cm/cm0.0060 - 0.0080 in/inISO 2577
Linear Mold Shrinkage, Transverse 0.0060 - 0.0080 cm/cm0.0060 - 0.0080 in/inISO 2577
Melt Index of Compound 9.0 g/10 min
@Load 5.00 kg,
Temperature 230 °C
9.0 g/10 min
@Load 11.0 lb,
Temperature 446 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break <= 48.0 MPa<= 6960 psiISO/R527
Elongation at Yield 6.0 %6.0 %ISO/R527
Flexural Strength <= 80.0 MPa<= 11600 psiISO 178
Flexural Modulus 2.30 GPa
@Temperature 23.0 °C
334 ksi
@Temperature 73.4 °F
ISO 178
Charpy Impact, Notched  0.900 J/cm²
@Temperature -20.0 °C
4.28 ft-lb/in²
@Temperature -4.00 °F
ISO 179
 1.30 J/cm²
@Temperature 23.0 °C
6.19 ft-lb/in²
@Temperature 73.4 °F
ISO 179
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 98.0 °C208 °F120°C/h; ISO 75/1
Deflection Temperature at 1.8 MPa (264 psi) 82.0 °C180 °F120°C/h; ISO 75/1
Vicat Softening Point  108 °C
@Load 5.001 kg
226 °F
@Load 11.03 lb
50°C/h; ISO 306
 118 °C
@Load 1.00 kg
244 °F
@Load 2.21 lb
50°C/h; ISO 306
Flammability, UL94 HB
@Thickness 1.60 mm
HB
@Thickness 0.0630 in
 
Processing PropertiesMetricEnglishComments
Melt Temperature 190 - 230 °C374 - 446 °F
Mold Temperature 60.0 - 80.0 °C140 - 176 °F
Drying Temperature 80.0 °C176 °F
Dry Time 2 - 4 hour2 - 4 hourin circulation dryer
 2 - 4 hour2 - 4 hourin fresh-air dryer
 2 - 4 hour2 - 4 hourin desiccant air dryer
Injection Pressure 90.0 - 150 MPa13100 - 21800 psi
Back Pressure 1.00 - 1.50 MPa145 - 218 psi
 
Descriptive Properties
Holding Pressure20-40% of injection pressure
Injection SpeedHigh

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Avient Elastamax™ EG-9077 Thermoplastic Elastomer (TPE)
Polykemi AB POLYabs H00 ABS, Heat Resistant
OJSC Plastic ABS 1030-31 ABS Plastic
LG Chemical XG568 MABS, Anti-Scratch, High Gloss
LG Chemical HF380I ABS, High Flow

PPOLYK164 / 122889

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.