MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Ineos R35C-02 Polypropylene Random Copolymer
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene Copolymer

Material Notes: Grade R35C-02 is a high clarity, lubricated random copolymer with a high flow rate. This material is designed for high-speed injection molding of medium- to thin-walled parts requiring excellent clarity, fast cycle times, and ease of denesting. Finished parts made with R35C-02 will exhibit a bluish hue giving a look of enhanced clarity. This material meets the requirements of the U.S. Food and Drug Administration as specified in 21 CFR 177.1520.
    Applications:
  • Medium- to thin-walled injection molding of multi-cavity parts
  • Housewares and consumer products – especially storage bins, containers and cups
  • Audio and video media rigid packaging
    Benefits:
  • High flow rate
  • Fast cycling time
  • Excellent clarity
  • Excellent mold release and denesting of parts
  • Good impact resistance

    Information provided by Ineos Olefins & Polymers USA

Key Words: High clarity, lubricated random copolymer with a high flow rate
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.906 g/ccASTM D792
Melt Flow 35 g/10 min
@Load 2.16 kg,
Temperature 230 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 83ASTM D785
Tensile Strength at Break 2500 psi2.0 in/min; ASTM D638
Tensile Strength, Yield 4260 psi2.0 in/min; ASTM D638
Elongation at Break >= 500 %2.0 in/min; ASTM D638
Elongation at Yield 14 %2.0 in/min; ASTM D638
Flexural Modulus, 1% Secant 156000 psiASTM D790A
Izod Impact, Notched 0.600 ft-lb/in
@Temperature 3.89 °C
ASTM D256
 1.10 ft-lb/in
@Temperature 22.8 °C
ASTM D256
Izod Impact, Notched (ISO) 1.50 ft-lb/in²
@Temperature 3.89 °C
Area; ASTM D256
 2.85 ft-lb/in²
@Temperature 22.8 °C
Area; ASTM D256
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 172 °FUnannealed; ASTM D648
Vicat Softening Point 266 °FASTM D1525
 
Optical PropertiesOriginal ValueComments
Haze 17 %
@Thickness 1.27 mm
ASTM D1003
Gloss 96 %60°; ASTM D2457
Transmission, Visible 14.3 %
@Thickness 1.27 mm
As molded, plaque, Diffuse Transmittance; ASTM D1003
 16.4 %
@Thickness 1.27 mm
ASTM standard conditioning, plaque, Diffuse Transmittance; ASTM D1003
 
Compliance PropertiesOriginal ValueComments
FDA YesSee notes for details.
 
Descriptive Properties
ProcessInjection Molding

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Ineos R35C-01 Polypropylene Random Copolymer
Ineos H12G-01 Polypropylene Homopolymer
Ineos N12N-00 Polypropylene Impact Copolymer
Ineos R35C-00 Polypropylene Random Copolymer
Phillips 66 COPYLENE® CR350CS-01 Polypropylene Random Copolymer

PINEOS910 / 130369

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.