MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Hexcel® HexPly® F155 Epoxy Resin
Categories: Polymer; Thermoset; Epoxy; Epoxy Cure Resin

Material Notes: HexPly® F155 is an advanced modified epoxy formulation designed for autoclave curing to offer very high laminate strengths, coupled with increased fracture toughness and adhesive properties. HexPly® F155 is a controlled flow epoxy resin for lamination and co-curing at 250ºF (121ºC) cure. HexPly® F155 will pass MIL-R-9300, co-cure as a honeycomb facing, and bond metal to metal.

Information provided by HexCel

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.335 g/cc
Moisture Absorption at Equilibrium 9.4 %
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 80.0 MPa
Elongation at Yield 5.2 %
Tensile Modulus 3.24 GPa
Fracture Toughness 1.65 MPa-m½
 
Thermal PropertiesOriginal ValueComments
CTE, linear 52.7 µm/m-°C
Glass Transition Temp, Tg 121 °CDry
 
Processing PropertiesOriginal ValueComments
Gel Time 4.00 - 10.0 min
@Temperature 121 °C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Hexcel® F161 Epoxy Resin
Hexcel® HexPly® F185 Epoxy Resin
Master Bond EP112M Two Component, Medium Viscosity Heat Curing Cycloaliphatic Epoxy Resin
Hexcel® HexPly® F155 Epoxy Resin, K120 Kevlar Fabric
Solvay CYCOM® 7701 Epoxy - Crowfoot Satin Fabric Composite

PHEXC095 / 98565

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.