MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

LyondellBasell Petrothene® NA860241 Low Density Polyethylene  (discontinued **)
Categories: Polymer; Thermoplastic; Polyethylene (PE); Low Density (LDPE); Low Density Polyethylene (LDPE), Molded

Material Notes: Applications
PETROTHENE NA 860 is a series of medium flow, low density polyethylene resins for the injection molding of caps, closures and other specialty applications. These resins exhibit an excellent balance of toughness, softness, dimensional stability and processability.

Regulatory Status
NA 860 meets the requirements of the Food and Drug Administration regulation, 21 CFR 177.1520. This regulation allows the use of this olefin polymer in "…articles or components of articles intended for use in contact with food…" Specific limitations or conditions of use may apply.

Processing Techniques
Specific recommendations for processing NA 860 can only be made when the processing conditions, equipment and end use are known.

This product is from the former Equistar product line.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.922 g/cc0.0333 lb/in³ASTM D1505
Melt Flow 25 g/10 min25 g/10 minASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 4444ASTM D2280
Tensile Strength at Break 8.48 MPa1230 psiCrosshead Speed - 20 in/min; ASTM D638
Tensile Strength, Yield 12.2 MPa1770 psiCrosshead Speed - 20 in/min; ASTM D638
Elongation at Yield 14 %14 %Crosshead Speed - 20 in/min; ASTM D638
Flexural Modulus, 1% Secant 221 MPa32000 psiCrosshead Speed - 1/2 in/min; ASTM D790
2% Secant Modulus 0.179 GPa26.0 ksiCrosshead Speed - 1/2 in/min; ASTM D790
 
Thermal PropertiesMetricEnglishComments
Vicat Softening Point 92.0 °C198 °FASTM D1525
Brittleness Temperature -35.0 °C-31.0 °FF50, Test method has been found useful for specification purposes, but does not necessarily indicate the lowest temperature at which the material may be used.; ASTM D746
 
Compliance PropertiesMetricEnglishComments
FDA YesYesSee notes for details.
 
Descriptive Properties
AntioxidantLow
SlipHigh

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PEQU0545b / 37015

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.