MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Polykemi AB POLYfill PP CQX10030E10 Polypropylene, Mineral Reinforced, Elastomer Modified
Categories: Polymer; Thermoplastic; Polypropylene (PP)

Material Notes:

Information provided by Polykemi AB

Key Words: Polypropylene, PP
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.10 g/cc0.0397 lb/in³ISO 1183
Filler Content 30 %30 %±2%; Polykemi
Linear Mold Shrinkage, Flow 0.012 - 0.014 cm/cm0.012 - 0.014 in/inISO 2577
Linear Mold Shrinkage, Transverse 0.012 - 0.014 cm/cm0.012 - 0.014 in/inISO 2577
Melt Index of Compound 10 g/10 min
@Load 2.16 kg,
Temperature 230 °C
10 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break <= 19.0 MPa<= 2760 psiISO/R527
Elongation at Break 23 %23 %ISO/R527
Elongation at Yield 7.0 %7.0 %ISO/R527
Flexural Strength <= 35.0 MPa<= 5080 psiISO 178
Flexural Modulus 1.70 GPa
@Temperature 23.0 °C
247 ksi
@Temperature 73.4 °F
ISO 178
Charpy Impact Unnotched  4.50 J/cm²
@Temperature -20.0 °C
21.4 ft-lb/in²
@Temperature -4.00 °F
ISO 179
 NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
ISO 179
Charpy Impact, Notched  0.400 J/cm²
@Temperature -20.0 °C
1.90 ft-lb/in²
@Temperature -4.00 °F
ISO 179
 1.00 J/cm²
@Temperature 23.0 °C
4.76 ft-lb/in²
@Temperature 73.4 °F
ISO 179
 
Thermal PropertiesMetricEnglishComments
CTE, linear 70.0 - 90.0 µm/m-°C38.9 - 50.0 µin/in-°FPolykemi
Deflection Temperature at 0.46 MPa (66 psi) 111 °C232 °F120°C/h; ISO 75/1
Deflection Temperature at 1.8 MPa (264 psi) 58.0 °C136 °F120°C/h; ISO 75/1
Vicat Softening Point  70.0 °C
@Load 5.001 kg
158 °F
@Load 11.03 lb
50°C/h; ISO 306
 144 °C
@Load 1.00 kg
291 °F
@Load 2.21 lb
50°C/h; ISO 306
Glow Wire Test 750 °C
@Thickness 2.00 mm
1380 °F
@Thickness 0.0787 in
IEC 695-2-1
 
Processing PropertiesMetricEnglishComments
Melt Temperature 230 - 250 °C446 - 482 °F
Mold Temperature 40.0 - 60.0 °C104 - 140 °F
Drying Temperature 70.0 - 80.0 °C158 - 176 °F
Dry Time 2 - 4 hour2 - 4 hourin circulation dryer
 2 - 4 hour2 - 4 hourin desiccant air dryer
Injection Pressure 40.0 - 70.0 MPa5800 - 10200 psi
Back Pressure 1.00 - 1.50 MPa145 - 218 psi
 
Descriptive Properties
Holding Pressure> 40% of injection pressure
Injection SpeedHigh
Scratch Resistance, 10N (dL)< 0.110 N Fine structure; ISO 1518/D65

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PPOLYK136 / 122861

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.