Azoty Tarnow™ TARNOFORM 300 HI6 POM
Categories:
Polymer
;
Thermoplastic
;
Acetal (Polyoxymethylene, POM)
;
Acetal Copolymer, Impact Modified
Material Notes:
Rubber modified grade with very high impact strength and damping capacity.
Information provided by Zakłady Azotowe w Tarnowie-Moscicach S.A.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
1.33
g/cc
0.0480
lb/in³
ISO 1183
Linear Mold Shrinkage
0.0265
cm/cm
0.0265
in/in
Melt Flow
5.0
g/10 min
@Load 2.16 kg,
Temperature 190 °C
5.0
g/10 min
@Load 4.76 lb,
Temperature 374 °F
ISO 1133
Mechanical Properties
Metric
English
Comments
Hardness, Rockwell R
87
87
ISO 2039-2
Ball Indentation Hardness
52.0
MPa
7540
psi
132 N; ISO 2039-1
Tensile Strength, Yield
32.0
MPa
4640
psi
ISO 527
Elongation at Break
180 %
180 %
ISO 527
Flexural Strength
27.0
MPa
3920
psi
ISO 178
Izod Impact, Notched (ISO)
17.0
kJ/m²
8.09
ft-lb/in²
1A; ISO 180
Charpy Impact, Notched
1.80
J/cm²
8.57
ft-lb/in²
1eA; ISO 179
Electrical Properties
Metric
English
Comments
Volume Resistivity
1.00e+14
ohm-cm
1.00e+14
ohm-cm
IEC 60093
Surface Resistance
1.00e+14
ohm
1.00e+14
ohm
IEC 60093
Dielectric Constant
4.5
@Frequency 1e+6 Hz
4.5
@Frequency 1e+6 Hz
IEC 60250
Dielectric Strength
20.0
kV/mm
508
kV/in
IEC 60243
Dissipation Factor
0.0425
@Frequency 1e+6 Hz
0.0425
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index
600
V
600
V
IEC 112
Thermal Properties
Metric
English
Comments
Specific Heat Capacity
1.48
J/g-°C
0.354
BTU/lb-°F
Melting Point
167
°C
333
°F
10°C/min.; ISO 3146
Deflection Temperature at 1.8 MPa (264 psi)
67.0
°C
153
°F
ISO 75
Vicat Softening Point
99.0
°C
210
°F
50 N; ISO 306
Flammability, UL94
HB
@Thickness 3.20 mm
HB
@Thickness 0.126 in
Processing Properties
Metric
English
Comments
Processing Temperature
180
-
210
°C
356
-
410
°F
Barrel temperature
Mold Temperature
50.0
-
80.0
°C
122
-
176
°F
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
PZAK021 / 72860
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.