MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metal adhesives

3M Scotch-Weld™ DP825 Acrylic Adhesives
Categories: Polymer; Adhesive; Thermoset; Acrylic/Cyanoacrylate Adhesive

Material Notes: 3M™ Scotch-Weld™ Acrylic Adhesive DP825 is a two-part, 1:1 mix ratio, toughened acrylic structural adhesives. They exhibit excellent shear and peel strengths along with good impact, durability and bond well to many metals, ceramics, wood and most plastics with minimal surface preparation.

Information provided by 3M

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Viscosity >= 3500 cP>= 3500 cPBase
 >= 7500 cP>= 7500 cPAccelerator
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 7070
Shear Strength 5.52 MPa800 psiOverlap, Etched Aluminum tested after 1 week of Immersion in Toluene
 6.55 MPa950 psiOverlap, Acrylic, Substrate Failure
 6.89 MPa1000 psiOverlap, Etched Aluminum
 7.067 MPa1025 psiOverlap, PC, Substrate Failure
 7.24 MPa1050 psiOverlap, ABS, Substrate Failure
 9.65 MPa1400 psiOverlap, PVC, Substrate Failure
 15.00 MPa2175 psiOverlap, Etched Aluminum tested after 1 week of Immersion in 66°C tap water
 17.41 MPa2525 psiOverlap, Etched Aluminum tested after 1 week of Immersion in Unleaded gasoline
 17.9 MPa2600 psiOverlap, Cold-Rolled Steel - slightly oily, Cohesive Failure
 18.10 MPa2625 psiOverlap, Green Fiberglass Reinforced Plastic, Adhesive Failure
 18.10 MPa2625 psiOverlap, Etched Aluminum
 18.44 MPa2675 psiOverlap, Etched Aluminum
 20.86 MPa3025 psiOverlap, Cold-Rolled Steel - solvent cleaned, Adhesive Failure
 26.37 MPa3825 psiOverlap, Etched Aluminum tested after 1 week of Immersion in IPA
 26.5 MPa3850 psiOverlap, Aluminum - etched, Adhesive Failure
 26.72 MPa3875 psiOverlap, Stainless Steel, Adhesive Failure
 27.06 MPa3925 psiOverlap, Aluminum - abraded, 150 grit sandpaper, Adhesive Failure
 28.3 MPa4100 psiOverlap, Aluminum - bare, Adhesive Failure
 30.3 MPa4400 psiOverlap, Etched Aluminum tested after 1 week of Immersion in Diesel fuel
 30.85 MPa4475 psiOverlap, Etched Aluminum
 32.1 MPa4650 psiOverlap, Etched Aluminum tested after 1 week of Immersion in 50% Antifreeze
 33.1 MPa4800 psiOverlap, Etched Aluminum cured for 7 days @ RT
 33.4 MPa4850 psiOverlap, Etched Aluminum tested after 1 week of Immersion in 20% bleach solution
 46.9 MPa6800 psiOverlap, Etched Aluminum tested after 1 week of Immersion in 66°C and 80% RH
Peel Strength 4.91 kN/m28.0 pliEtched Al/Etched Al after 1 week at RT cure
 
Processing PropertiesMetricEnglishComments
Cure Time 240 - 1440 min4.00 - 24.0 hourFull cure
 
Descriptive Properties
AppearanceOff-whiteBase
 Pale yellow
 YellowAccelerator

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
DuPont Teijin Films Mylar® HP Polyester Film, 36 Gauge
DuPont Teijin Films Mylar® ADS Polyester Film, 300 Gauge
DuPont Teijin Films Mylar® A Polyester Film, 48 Gauge
DuPont Teijin Films Mylar® 851H Polyester Film, 60 Gauge
3M Scotch-Weld™ DP820 Acrylic Adhesives

PMM34598 / 169345

Metal adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.