Physical Properties | Metric | English | Comments |
---|
Density | 1.48 g/cc | 0.0535 lb/in³ |
Filler Content | 30 % | 30 % |
Moisture Absorption | 0.60 - 0.70 % @Temperature 70.0 °C | 0.60 - 0.70 % @Temperature 158 °F |
| 0.400 % @Time 90000 sec | 0.400 % @Time 25.0 hour |
| 0.650 % @Time 180000 sec | 0.650 % @Time 50.0 hour |
| 0.700 % @Time 900000 sec | 0.700 % @Time 250 hour |
| 0.700 % @Time 1.62e+6 sec | 0.700 % @Time 450 hour |
Linear Mold Shrinkage, Flow | 0.0070 cm/cm | 0.0070 in/in |
Linear Mold Shrinkage, Transverse | 0.013 cm/cm | 0.013 in/in |
|
Mechanical Properties | Metric | English | Comments |
---|
Tensile Strength at Break | 130 MPa | 18900 psi |
Tensile Stress | 33.0 MPa @Temperature 150 °C | 4790 psi @Temperature 302 °F |
| 41.0 MPa @Temperature 120 °C | 5950 psi @Temperature 248 °F |
| 47.0 MPa @Temperature 80.0 °C | 6820 psi @Temperature 176 °F |
| 52.0 MPa @Temperature 150 °C | 7540 psi @Temperature 302 °F |
| 58.0 MPa @Temperature 150 °C | 8410 psi @Temperature 302 °F |
| 65.0 MPa @Temperature 23.0 °C | 9430 psi @Temperature 73.4 °F |
| 65.0 MPa @Temperature 120 °C | 9430 psi @Temperature 248 °F |
| 80.0 MPa @Temperature 80.0 °C | 11600 psi @Temperature 176 °F |
| 102 MPa @Temperature 23.0 °C | 14800 psi @Temperature 73.4 °F |
| 122 MPa @Temperature 23.0 °C | 17700 psi @Temperature 73.4 °F |
Elongation at Break | >= 3.0 % | >= 3.0 % |
Tensile Modulus | 7.50 GPa | 1090 ksi |
Flexural Modulus | 8.30 GPa | 1200 ksi |
Charpy Impact Unnotched | 6.00 J/cm² @Temperature 23.0 °C | 28.6 ft-lb/in² @Temperature 73.4 °F |
Charpy Impact, Notched | 1.50 J/cm² @Temperature 23.0 °C | 7.14 ft-lb/in² @Temperature 73.4 °F |
Coefficient of Friction, Dynamic | 0.50 | 0.50 |
K (wear) Factor | 14.5 x 10-8 mm³/N-M | 7.20 x 10-10 in³-min/ft-lb-hr |
|
Electrical Properties | Metric | English | Comments |
---|
Volume Resistivity | 1.00e+12 ohm-cm | 1.00e+12 ohm-cm |
Surface Resistance | 1.00e+13 ohm | 1.00e+13 ohm |
|
Thermal Properties | Metric | English | Comments |
---|
Melting Point | 220 °C | 428 °F |
Deflection Temperature at 0.46 MPa (66 psi) | 220 °C | 428 °F |
Deflection Temperature at 1.8 MPa (264 psi) | 215 °C | 419 °F |
Flammability, UL94 | HB @Thickness 1.60 mm | HB @Thickness 0.0630 in |
|
Processing Properties | Metric | English | Comments |
---|
Feed Temperature | 60.0 - 80.0 °C | 140 - 176 °F |
Nozzle Temperature | 230 - 250 °C | 446 - 482 °F |
Zone 1 | 210 - 250 °C | 410 - 482 °F |
Zone 2 | 210 - 250 °C | 410 - 482 °F |
Zone 3 | 210 - 250 °C | 410 - 482 °F |
Zone 4 | 210 - 250 °C | 410 - 482 °F |
Melt Temperature | 230 - 250 °C | 446 - 482 °F |
Mold Temperature | 60.0 - 80.0 °C | 140 - 176 °F |
Drying Temperature | 60.0 - 80.0 °C | 140 - 176 °F |
Dry Time | <= 4.00 hour | <= 4.00 hour |
Back Pressure | 30.0 - 80.0 MPa | 4350 - 11600 psi |
|
Descriptive Properties |
---|
Resistance to Acetic Acid | 1% Change in Volume |
| 1% Change in Volume |
| 3% Change in Weight |
| 3% Change in Weight |
Resistance to Acetone | 2% Change in Volume |
| 5% Change in Volume |
| 5% Change in Weight |
| 5% Change in Weight |
Resistance to Ammonium hydroxide 10% | 0% Change in Volume |
| 0% Change in Weight |
| -3% Change in Volume |
| -5% Change in Weight |
Resistance to Antifreeze 50%, 50% water | 0% Change in Volume |
| 0% Change in Weight |
| 1% Change in Volume |
| 1% Change in Weight |
Resistance to Antifreeze, 100% ethylene glycol | 0% Change in Volume |
| 0% Change in Weight |
| 5% Change in Volume |
| 5% Change in Weight |
Resistance to Automatic transmission fluid | 0% Change in Volume |
| 0% Change in Volume |
| 0% Change in Weight |
| 0% Change in Weight |
Resistance to Brake fluid | 0% Change in Volume |
| 0% Change in Weight |
| 5% Change in Volume |
| 5% Change in Weight |
Resistance to Butyl acetate | 0% Change in Volume |
| 0% Change in Weight |
| 2% Change in Volume |
| 2% Change in Weight |
Resistance to Calcium Chloride | 0% Change in Volume |
| 0% Change in Weight |
Resistance to Chassis lube | 0% Change in Volume |
| 0% Change in Weight |
| -1% Change in Volume |
| -1% Change in Weight |
Resistance to Dichloroethane | 0% Change in Volume |
| 0% Change in Weight |
Resistance to Dimethyl formamide | 0% Change in Volume |
| 2% Change in Weight |
| Samples swell and slowly dissolve |
| Samples swell and slowly dissolve |
Resistance to Ethanol | 1% Change in Volume |
| 2% Change in Volume |
| 2% Change in Weight |
| 2% Change in Weight |
Resistance to Gasohol (unleaded, 10% methanol) | 0% Change in Volume |
| 1% Change in Weight |
| 3% Change in Weight |
| 5% Change in Volume |
Resistance to Gasohol M-25 (unleaded, 15% methanol) | 0% Change in Volume |
| 1% Change in Weight |
| 3% Change in Volume |
| 5% Change in Weight |
Resistance to Heptane | 0% Change in Volume |
| 0% Change in Volume |
| 0% Change in Weight |
| 0% Change in Weight |
Resistance to Hydraulic fluid | 0% Change in Volume |
| 0% Change in Volume |
| 0% Change in Weight |
| 0% Change in Weight |
Resistance to Hydrochloric acid | 0% change in volume |
| 0% change in volume |
| 2% change in weight |
| 2% change in weight |
Resistance to Jet fuel A | 0% Change in Volume |
| 0% Change in Weight |
| 1% Change in Weight |
| 2% Change in Volume |
Resistance to Methanol | 1% Change in Volume |
| 2% Change in Weight |
| 2% Change in Weight |
| 3% Change in Volume |
Resistance to Methylethylketone | 2% Change in Volume |
| 2% Change in Weight |
Resistance to Motor oil (SAE 10W-40) | 0% Change in Volume |
| 0% Change in Weight |
| 0% Change in Weight |
| -1% Change in Volume |
Resistance to MTBE | 1% Change in Volume |
| 1% Change in Weight |
Resistance to Sodium Chloride 10% | 0% Change in Volume |
| 0% Change in Weight |
| 0% Change in Weight |
| -1% Change in Volume |
Resistance to Sodium hydroxide 10% | 0% Change in Volume |
| 1% Change in Weight |
| 5% Change in Volume |
| 5% Change in Weight |
Resistance to Sodium hypochlorite 4.6% | -1% Change in Volume |
| -1% Change in Volume |
| -1% Change in Weight |
| -2% Change in Weight |
Resistance to Sulfuric acid | 0% change in volume |
| 0% change in volume |
| 0% change in weight |
| -1% change in volume |
| -1% change in volume |
| 1% change in weight |
| -1% change in weight |
| -1% change in weight |
Resistance to Tetrachloroethylene | 0% Change in Volume |
| 1% Change in Weight |
| 2% Change in Volume |
| 3% Change in Weight |
Resistance to Toluene | 0% Change in Volume |
| 1% Change in Volume |
| 1% Change in Weight |
| 4% Change in Weight |
Resistance to Trichlorethane | 0% Change in Volume |
| 1% Change in Volume |
| 1% Change in Weight |
| 5% Change in Weight |
Resistance to Unleaded gasoline | 0% Change in Volume |
| 0% Change in Weight |
| 1% Change in Weight |
| 3% Change in Volume |
Resistance to Xylene | 0% Change in Volume |
| 0% Change in Weight |
Resistance to Zinc chloride 10% | 2% Change in Weight |
| 3% Change in Volume |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.