MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

Supreme Petrochem SP 6520 Permanent Antistatic Polystyrene
Categories: Polymer; Thermoplastic; Polystyrene (PS); Polystyrene, Molded, Unreinforced

Material Notes: Characteristics
  • No sloughing
  • Fully colorable
  • Meets MIL-PRF-81705D static decay specification
  • Functions even in low humidity levels
Processing
  • Injection molding
  • Extrusion & Forming
Applications
  • Component handling systems
  • Chip trays
  • ESD applications
  • PCB boxes
  • Component boxes
Material Status: Commercial : Active

Agency Ratings:

Information provided by Supreme Petrochem LTD

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.05 g/cc1.05 g/ccASTM D792
Melt Flow 3.0 g/10 min
@Load 5.00 kg,
Temperature 200 °C
3.0 g/10 min
@Load 11.0 lb,
Temperature 392 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 27.0 MPa3920 psi50 mm/min; ASTM D638
Elongation at Break 4.0 %4.0 %50 mm/min; ASTM D638
Flexural Strength 43.1 MPa
@Thickness 3.20 mm
6250 psi
@Thickness 0.126 in
ASTM D790
Flexural Modulus 1.47 GPa
@Thickness 3.20 mm
213 ksi
@Thickness 0.126 in
ASTM D790
Izod Impact, Notched 0.550 J/cm
@Thickness 3.20 mm
1.03 ft-lb/in
@Thickness 0.126 in
ASTM D256
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+9 - 1.00e+10 ohm-cm1.00e+9 - 1.00e+10 ohm-cmASTM D257
Surface Resistance 1.00e+9 - 1.00e+10 ohm1.00e+9 - 1.00e+10 ohmASTM D257
Static Decay <= 2.0 sec<= 2.0 secMIL-PRF-81705D
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 1.8 MPa (264 psi) 81.0 °C178 °FASTM D648
Vicat Softening Point 98.0 °C208 °F1kg load; 120°C/h; ASTM D1525
Flammability, UL94 HB
@Thickness 1.60 mm
HB
@Thickness 0.0630 in
 
Processing PropertiesMetricEnglishComments
Melt Temperature <= 230 °C<= 446 °F
Mold Temperature 40.0 - 60.0 °C104 - 140 °F
Drying Temperature 60.0 - 80.0 °C140 - 176 °F( 2 hrs) Pre drying temp.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSUP36 / 69468

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.