MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Asahi Kasei DELPET™ 60N Acrylic (PMMA), Standard Grade
Categories: Polymer; Thermoplastic; Acrylic (PMMA); Acrylic, General Purpose, Molded

Material Notes: 60N is a medium grade of heat resistance and mechanical strength, allowing injection molding through relatively small gates and runners.

DELPET™ has excellent transparency, surface hardness and weatherability. Main applications of DELPET™ are outer/inner parts for automobile, optical goods, industrial and general parts/goods.

Information provided by Asahi Kasei Corp.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.19 g/cc1183
Water Absorption 0.30 %
@Temperature 23.0 °C
ISO 62 Method 1
Linear Mold Shrinkage 0.0020 - 0.0060 cm/cmAsahiKasei Method
Melt Flow 8.0 g/10 min
@Load 3.80 kg,
Temperature 230 °C
1133, cond 13
Spiral Flow 38.0 cm
@Thickness 2.00 mm,
Pressure 75.0 MPa
cylinder temp 250°C, mold temp 60°C; AsahiKasei Method
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 952039-2
Tensile Strength at Break 72.0 MPa527-2/1A/5
Elongation at Break 5.0 %527-2/1A/5
Tensile Modulus 3300 MPa527-2/1A/1
Flexural Strength 120 MPa178
Flexural Modulus 3300 MPa178
Charpy Impact Unnotched 20.0 kJ/m²179/1eU
Charpy Impact, Notched 1.30 kJ/m²179/1eA
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 91.0 °CDeflection Temperature, load not reported; ISO 75-1
Vicat Softening Point 98.0 °C306 B50
 
Optical PropertiesOriginal ValueComments
Refractive Index 1.49489
UV Transmittance 92 %13468-1

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Trinseo Plexiglas® V044 Acrylic
Asahi Kasei DELPET™ 560F Acrylic (PMMA), Standard Grade
Arkema Oroglas® MI-4T Acrylic, Heat Resistant
LG Chemical IH830C PMMA, General Purpose Grade for Injection Molding
Trinseo Plexiglas® V052 Acrylic

PASAHI8006 / 221033

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.