MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Elix Polymers Elix™ P2H-AT ABS Polymer
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylonitrile Butadiene Styrene (ABS), Molded

Material Notes: Standard impact strength, easy flowing, high gloss, contains antistatic additives. Main Applications: Household appliances, Housings (phone, computer, printer). Automotive interior, Automotive exterior, Toys, Cosmetics packaging, Extruded sheets, Medical devices, Electroplating, Pipes, Covers, Smart cards.

Property data measured at 23°C and 50% RH.

Information provided by Elix Polymers.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.05 g/ccISO 1183
Linear Mold Shrinkage, Flow 0.0040 - 0.0060 cm/cm
@Thickness 2.00 mm
60 X 60 mm; ISO-294-4
Linear Mold Shrinkage, Transverse 0.0040 - 0.0060 cm/cm
@Thickness 2.00 mm
60 X 60 mm; ISO-294-4
Melt Flow 37 g/10 min
@Load 10.0 kg,
Temperature 220 °C
cm³/10 min MVR; ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Ball Indentation Hardness 110 MPaISO 2039-1
Tensile Strength, Yield 44.0 MPa50 mm/min; ISO 527-1,2
Elongation at Break >= 15 %50 mm/min; acc. ISO 527-1,2
Elongation at Yield 2.1 %50 mm/min; ISO 527-1,2
Tensile Modulus 2500 MPa1mm/min.; ISO 527-1,2
Flexural Strength 70.0 MPa2mm/min; ISO 178
Flexural Modulus 2400 MPa2mm/min; ISO 178
Izod Impact, Notched (ISO) 7.00 kJ/m²
@Temperature -30.0 °C
ISO 180-1A
 16.0 kJ/m²
@Temperature 23.0 °C
ISO 180-1A
Charpy Impact Unnotched 80.0 kJ/m²
@Temperature -30.0 °C
ISO 179-1eU
 100 kJ/m²
@Temperature 23.0 °C
ISO 179-1eU
Charpy Impact, Notched 7.00 kJ/m²
@Temperature -30.0 °C
ISO 179-1eA
 16.0 kJ/m²
@Temperature 23.0 °C
ISO 179-1eA
Tensile Creep Modulus, 1 hour 2200 MPaISO 899-1
Tensile Creep Modulus, 1000 hours 1500 MPaISO 899-1
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+15 ohm-cmIEC 60093
Surface Resistance 1.00e+15 ohmIEC 60093
Dielectric Constant 2.9
@Frequency 1e+6 Hz
IEC 60250
 3.0
@Frequency 100 Hz
IEC 60250
Dielectric Strength 34.0 kV/mm
@Thickness 1.00 mm
IEC 60243-1
Dissipation Factor 0.0055
@Frequency 100 Hz
IEC 60250
 0.0090
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 600 Vsolution A; IEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 90.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
ISO 11359-1,2
Deflection Temperature at 0.46 MPa (66 psi) 97.0 °CISO 75-1,2
Deflection Temperature at 1.8 MPa (264 psi) 93.0 °CISO 75-1,2
Vicat Softening Point 98.0 °C50N 50°C/h; ISO 306
Flammability, UL94 HB
@Thickness 1.60 mm
Flammability Test 60
@Thickness 2.00 mm
US-FMVSS , mm/min; ISO 3795
Glow Wire Flammability Index 700 °C
@Thickness 2.00 mm
IEC 60695-2,12
 
Processing PropertiesOriginal ValueComments
Melt Temperature 240 °Cinjection molding; ISO 294
Mold Temperature 70.0 °Cinjection molding; ISO 294
Injection Velocity 240 mm/secinjection molding; ISO 294

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
INEOS Styrolution Terluran® GP-35 ABS
Lotte Advanced Materials Starex® HG-0760 ABS, Unreinforced
Elix Polymers ELIX ABS P2H-AT Acrylonitrile Butadiene Styrene (ABS)
Chi Mei Polylac® PA-709 ABS
Elix Polymers ELIX ABS P2M-AT Acrylonitrile Butadiene Styrene (ABS), High Impact Strength

PELIX901 / 192496

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.