MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Teknor Apex Sarlink® TPE EE-2365B Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes: Notes: Sarlink EE-2300 series is a high performance thermoplastic elastomer series, available in BLK, designed for demanding automotive low gloss extrusion applications including functional lip seals. Sarlink EE-2365B is a medium hardness, high density, filled, UV stabilized grade with exceptional tensile strength, superior surface aesthetics, good chemical resistance and good elasticity.

Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North America

Features: Chemical Resistant; Good Adhesion; Good Flexibility; Good Processability; Good Scratch Resistance; High Density; High Melt Stability; High Specific Gravity; High Tensile Strength; Low Gloss; Medium Hardness; Outstanding Surface Finish; UV Resistant

Uses: Automotive Applications; Automotive Exterior Parts; Profiles; Rubber Replacement; Seals; Weatherstripping

RoHS Compliance: RoHS Compliant

Form: Pellets

Processing Method: Extrusion; Coextrusion

Preliminary data. Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.12 g/cc0.0405 lb/in³ASTM D792
Viscosity 250 cP
@Shear Rate 206 1/s,
Temperature 200 °C
250 cP
@Shear Rate 206 1/s,
Temperature 392 °F
ASTM D3835
Melt Flow 4.0 g/10 min
@Load 5.00 kg,
Temperature 230 °C
4.0 g/10 min
@Load 11.0 lb,
Temperature 446 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 61
@Time 5.00 sec
61
@Time 0.00139 hour
Injection Molded; ISO 868
 65
@Treatment Temp. 125 °C,
Time 605000 sec
65
@Treatment Temp. 257 °F,
Time 168 hour
Change in Air; ISO 888
 65.1
@Treatment Temp. 110 °C,
Time 3.629e+6 sec
65.1
@Treatment Temp. 230 °F,
Time 1008 hour
Change in Air; ISO 888
Tensile Strength at Break 6.76 MPa980 psiFlow; ISO 37
 7.58 MPa1100 psiAcross Flow; ISO 37
Tensile Stress at Strain  2.10 MPa
@Strain 100 %
305 psi
@Strain 100 %
Across Flow; ISO 37
 2.60 MPa
@Strain 100 %
377 psi
@Strain 100 %
Flow; ISO 37
Elongation at Break 540 %540 %Flow; ISO 37
 690 %690 %Across Flow; ISO 37
 588 %
@Treatment Temp. 110 °C,
Time 3.629e+6 sec
588 %
@Treatment Temp. 230 °F,
Time 1008 hour
Across Flow, Change in Air; ISO 188
 635 %
@Treatment Temp. 125 °C,
Time 605000 sec
635 %
@Treatment Temp. 257 °F,
Time 168 hour
Across Flow, Change in Air; ISO 188
Tear Strength 26.3 kN/m150 pliAcross Flow; ISO 34-1
 28.0 kN/m160 pliFlow; ISO 34-1
Compression Set  20 %
@Temperature 22.8 °C,
Time 79200 sec
20 %
@Temperature 73.0 °F,
Time 22.0 hour
ISO 815
 36 %
@Temperature 70.0 °C,
Time 79200 sec
36 %
@Temperature 158 °F,
Time 22.0 hour
ISO 815
 59 %
@Temperature 90.0 °C,
Time 252000 sec
59 %
@Temperature 194 °F,
Time 70.0 hour
ISO 815
 
Processing PropertiesMetricEnglishComments
Zone 1 171 - 193 °C340 - 380 °F
Zone 2 177 - 199 °C350 - 390 °F
Zone 3 182 - 204 °C360 - 400 °F
Zone 4 182 - 204 °C360 - 400 °F
Zone 5 188 - 204 °C370 - 400 °F
Die Temperature 188 - 204 °C370 - 400 °F
Screw Speed 30 - 100 rpm30 - 100 rpm
 
Descriptive Properties
AppearanceBlack

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PTEKNQ1040 / 237531

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.