System Message
Advertise with MatWeb!
Data sheets for over
180,000
metals, plastics, ceramics, and composites.
HOME
•
SEARCH
•
TOOLS
•
SUPPLIERS
•
FOLDERS
•
ABOUT US
•
FAQ
•
LOG IN
Recently Viewed Materials (most recent at top)
Login
to see your most recently viewed materials here.
Or if you don't have an account with us yet, then
click here to register.
Searches:
Advanced
|
Category
|
Property
|
Metals
|
Trade Name
|
Manufacturer
|
Recently Viewed Materials
(Viewing data as-entered.
Click here
to return)
BASF Ultramid® FRee B3U31G4 20% Glass Filled PA66 FR (Dry)
Categories:
Polymer
;
Thermoplastic
;
Nylon (Polyamide PA)
;
Nylon 66 (PA66)
;
Nylon 66, 20% Glass Fiber Filled
Material Notes:
Description: Halogen-free and phosphorus free flame retardant injection-molding grade with outstanding free-flow properties, good electrical properties and low smoke density; resistant to glow wire test up to 960°C.
Information provided by BASF
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Original Value
Comments
Density
1.31
g/cc
ISO 1183
Moisture Absorption at Equilibrium
2.0 - 2.4 %
23°C; 50% RH; ISO 62
Water Absorption at Saturation
6.6 - 7.2 %
ISO 62
Melt Flow
131
g/10 min
@Load 5.00 kg,
Temperature 275 °C
ISO 1133
Mechanical Properties
Original Value
Comments
Tensile Strength, Yield
90.0
MPa
50 mm/min; ISO 527-1/-2
Elongation at Yield
2.8 %
50 mm/min; ISO 527-1/-2
Modulus of Elasticity
6.10
GPa
ISO 527-1/-2
Flexural Modulus
5700
MPa
ISO 178
Izod Impact, Notched (ISO)
3.00
kJ/m²
@Temperature -30.0 °C
ISO 180/A
3.50
kJ/m²
@Temperature 23.0 °C
ISO 180/A
Charpy Impact Unnotched
25.0
kJ/m²
@Temperature -30.0 °C
ISO 179/1eU
30.0
kJ/m²
@Temperature 23.0 °C
ISO 179/1eU
Charpy Impact, Notched
3.00
kJ/m²
@Temperature -30.0 °C
ISO 179/1eA
3.50
kJ/m²
@Temperature 23.0 °C
ISO 179/1eA
Electrical Properties
Original Value
Comments
Volume Resistivity
1.00e+14
ohm-cm
IEC 60093
Comparative Tracking Index
525
V
Test solution A; IEC 60112
Thermal Properties
Original Value
Comments
CTE, linear, Parallel to Flow
50.0
-
55.0
µm/m-°C
@Temperature 23.0 - 80.0 °C
DIN 11359-1/-2
CTE, linear, Transverse to Flow
50.0
-
60.0
µm/m-°C
@Temperature 23.0 - 80.0 °C
DIN 11359-1/-2
Melting Point
220
°C
DIN 53765
Deflection Temperature at 0.46 MPa (66 psi)
210
°C
ISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi)
165
°C
ISO 75-1/-2
Flammability, UL94
V-2
@Thickness >=0.710 mm
Processing Properties
Original Value
Comments
Melt Temperature
250
-
275
°C
Injection-molding/Extrusion
Mold Temperature
80.0
-
90.0
°C
Injection-molding
Descriptive Properties
Commercial Status
Europe
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to go back to viewing the property data in MatWeb's normal format.
Users viewing this material also viewed the following:
BASF Ultramid® FRee B3U31G4 20% Glass Filled PA66 FR (Conditioned)
BASF Ultramid® A3HG3 PA66 (Dry)
BASF Ultramid® A3HG3 PA66 (Conditioned)
Avient Edgetek® NN-20GF/000 Nylon 6/6, 20% Glass Fiber Reinforced
Asia International Enterprise (Hong Kong) 60G4 Nylon 66, 20% Filled
PBASG0326 / 131959
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.