MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Delrin Delrin® 100KM NC000 POM-RG
Categories: Polymer; Thermoplastic; Acetal (Polyoxymethylene, POM)

Material Notes: Kevlar® Modified High Viscosity Acetal Homopolymer with Low Wear and Low Friction

Information provided by DuPont; Delrin was sold by DuPont in 2023.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.41 g/ccISO 1183
Melt Density 1.18 g/cc
@Temperature 215 °C
Linear Mold Shrinkage, Flow 0.018 cm/cmISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.015 cm/cmISO 294-4, 2577
Melt Flow 1.7 g/10 min
@Load 2.16 kg,
Temperature 190 °C
cm³/10min Volumetric; ISO 1133
 2.0 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 65.0 MPaISO 527-1/-2
Elongation at Break 15 %ISO 527-1/-2
Tensile Modulus 3100 MPaISO 527-1/-2
Flexural Modulus 3000 MPaISO 178
Poissons Ratio 0.37
Charpy Impact Unnotched 50.0 kJ/m²
@Temperature 23.0 °C
ISO 179/1eU
 60.0 kJ/m²
@Temperature -30.0 °C
ISO 179/1eU
Charpy Impact, Notched 3.50 kJ/m²
@Temperature -30.0 °C
ISO 179/1eA
 4.50 kJ/m²
@Temperature 23.0 °C
ISO 179/1eA
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 110 µm/m-°CISO 11359-1/-2
 94.0 µm/m-°C
@Temperature -40.0 - 23.0 °C
ISO 11359-1/-2
CTE, linear, Transverse to Flow 100 µm/m-°CISO 11359-1/-2
 92.0 µm/m-°C
@Temperature -40.0 - 23.0 °C
ISO 11359-1/-2
Melting Point 178 °C10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 160 °CISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 98.0 °CISO 75-1/-2
Flame Spread 34.0 mm/min
@Thickness 1.00 mm
ISO 3795 (FMVSS 302)
 
Processing PropertiesOriginal ValueComments
Melt Temperature 195 - 205 °CRange, Extrusion
 200 °COptimum, Extrusion
 215 °COptimum, Injection
 210 - 220 °CRange, Injection
Mold Temperature 90.0 °COptimum, Injection
 80.0 - 100 °CInjection
Drying Temperature 80.0 °CInjection
 75.0 - 85.0 °CExtrusion
Dry Time 2.00 - 4.00 hourExtrusion, Dehumidified Dryer
 2.00 - 4.00 hourInjection, Dehumidified Dryer
Moisture Content <= 0.20 %Extrusion
 <= 0.20 %Injection
Hold Pressure 90.0 - 110 MPaInjection
 110 MPaInjection
Annealing Temperature 160 °COptional; 2 mm/min; Injection
 
Descriptive Properties
AdditivesRelease agent
Annealing time (min/mm)30Optional, Injection
Drying RecommendedyesInjection
FMVSS ClassBISO 3795 (FMVSS 302)
Max. screw tangential speed (m/s)0.2Injection
Part Marking Code>POM-AG10<ISO 11469
PolymerPOM-Z
Processing Hold Pressure Time (s/mm)8Injection
Resin IdentificationPOM-AG10ISO 1043

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Delrin Delrin® 100AF POM-PTFE20
Delrin Delrin® 100AL NC010 POM-S
Delrin Delrin® 100 NC010 POM
Delrin Delrin® 100P BK602 POM
Delrin Delrin® 100 BK602 POM

PDSX5084 / 197724

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.