MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

(Viewing data as-entered. Click here to return)
Aluminum 356.0-T7, Sand Cast
Categories: Metal; Nonferrous Metal; Aluminum Alloy; Aluminum Casting Alloy

Material Notes: Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
If iron exceeds 0.45%, manganese content shall not be less than one-half iron content.
Composition information provided by the Aluminum Association and is not for design.

Key Words: Aluminium 356.0-T7; UNS A03560; ISO 3522 and R2147 AlSi7Mg; AA356.0-T7. Comparable to JIS AC4C; Al356.0-T7
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.68 g/ccAA; Typical
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 60 - 90AA; Typical; 500 g load; 10 mm ball
Hardness, Knoop 98Estimated from Brinell Hardness.
Hardness, Vickers 85Estimated from Brinell Hardness.
Tensile Strength, Ultimate >= 31.0 ksiAA
Tensile Strength, Yield >= 29.0 ksi
@Strain 0.2 %
AA
Elongation at Break 2.0 %in 50 mm
Tensile Modulus 72.4 GPaCompressive modulus in is typically about 2% higher for Al alloys
Compressive Yield Strength 215 MPa
Poissons Ratio 0.33
Fatigue Strength 62.0 MPa
@# of Cycles 5.00e+8
Notch Status unknown, R.R. Moore Test
Machinability 50 %0-100 Scale (100=best)
Shear Modulus 27.2 GPa
Shear Strength 165 MPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000430 ohm-cmAA; Typical 40% IACS Conductivity
 
Thermal PropertiesOriginal ValueComments
Heat of Fusion 389 J/g
CTE, linear 11.9 µin/in-°F
@Temperature 20.0 - 100 °C
AA; Typical
 12.9 µin/in-°F
@Temperature 20.0 - 300 °C
AA; Typical; average over range
Specific Heat Capacity 0.963 J/g-°C
Thermal Conductivity 0.370 cal cm/sec-cm²-°CAA; Typical at 25°C
Melting Point 1035 - 1135 °FAA; Typical
Solidus 1035 °FAA; Typical
Liquidus 1135 °FAA; Typical
 
Processing PropertiesOriginal ValueComments
Melt Temperature 1250 - 1500 °F
Solution Temperature 995 - 1005 °Fhold at temperature for 12 hr; cool in water at 150 to 212°F
Aging Temperature 435 - 445 °Fhold at temperature 7 - 9 hrs; start with solution heat-treated material
Casting Temperature 1250 - 1450 °F
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 90.1 - 93.3 %As remainder
Copper, Cu <= 0.25 %
Iron, Fe <= 0.60 %
Magnesium, Mg 0.20 - 0.45 %
Manganese, Mn <= 0.35 %
Other, each <= 0.05 %
Other, total <= 0.15 %
Silicon, Si 6.5 - 7.5 %
Titanium, Ti <= 0.25 %
Zinc, Zn <= 0.35 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum 356.0-T6, Sand Cast
Aluminum 356.0-T51, Permanent Mold Cast
Aluminum 356.0-T71, Permanent Mold Cast
Aluminum 356.0-F, Permanent Mold Cast
Aluminum 356.0-F, Sand Cast

MAC3560T7S / 9937

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.