MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

(Viewing data as-entered. Click here to return)
Aluminum 6262-T6
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 6000 Series Aluminum Alloy

Material Notes: Information provided by Alcoa and the references. General 6262 characteristics and uses: Good machinability and high strength; high corrosion resistance and applied coating acceptance. Finishing characteristics better than 2011, 2017, 2024, 7075 and equal to 6061. The T8 temper offers excellent residual stress control.

Uses: Camera parts, couplings, marine fittings, decorative and misc. hardware, hinge pins, knobs, magneto parts, nuts, oil line fittings, appliance fittings, roller skate parts, steam iron parts, TV fittings, tripod fittings, valves and valve parts.

Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
Composition information provided by the Aluminum Association and is not for design.

Key Words: UNS A96262; ISO AlMg1SiPb; Aluminium 6262-T6; AA6262-T6; Al6262-T6
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 2.72 g/ccAA; Typical
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 71500 kg load with 10 mm ball
Hardness, Knoop 94Converted from Brinell Hardness Value
Hardness, Vickers 81Converted from Brinell Hardness Value
Tensile Strength, Ultimate 220 MPa
Tensile Strength, Yield 190 MPa
Modulus of Elasticity 69.0 GPaAverage of Tension and Compression. In Al alloys, the compressive modulus is typically 2% greater than the tensile modulus. Estimated from trends in similar Al alloys.
Poissons Ratio 0.33Estimated from trends in similar Al alloys.
Fatigue Strength 90.0 MPa
@# of Cycles 5.00e+8
unnotched R. R. Moore rotating beam
Machinability 70 %0-100 Scale of Aluminum Alloys
Shear Modulus 26.0 GPaEstimated from similar Al alloys.
Shear Strength 140 MPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000390 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 13.0 µin/in-°F
@Temperature 20.0 - 100 °C
AA; Typical; average over range
 25.0 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.890 J/g-°CEstimated from trends in similar Al alloys.
Thermal Conductivity 170 W/m-K
Melting Point 1080 - 1205 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness. Eutectic melting can be eliminated by homogenization.
Solidus 1080 °FAA; Typical
Liquidus 1205 °FAA; Typical
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 780 °Fhold at temperature 2 to 3 hr
Solution Temperature 1000 °Fhold at temperature 8 to 12 hr
Aging Temperature 340 °Fhold at temperature 8 to 12 hr
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 94.6 - 97.8 %As remainder
Bismuth, Bi 0.40 - 0.70 %
Chromium, Cr 0.04 - 0.14 %
Copper, Cu 0.15 - 0.40 %
Iron, Fe <= 0.70 %
Lead, Pb 0.40 - 0.70 %
Magnesium, Mg 0.80 - 1.2 %
Manganese, Mn <= 0.15 %
Other, each <= 0.05 %
Other, total <= 0.15 %
Silicon, Si 0.40 - 0.80 %
Titanium, Ti <= 0.15 %
Zinc, Zn <= 0.25 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum 6061-T6; 6061-T651
Aluminum 6262-T8
Aluminum 6262-T9
Aluminum 6082-T6
Aluminum 7075-T6; 7075-T651

MA6262T6 / 9485

Metalmen Sales

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.