MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
INEOS Styrolution Terblend® N NG-02 EF ABS+PA, 8% Glass Fiber Reinforced, Dry
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylonitrile Butadiene Styrene (ABS)/Nylon Blend, Glass Reinforced

Material Notes: Product Description: Terblend® N NG-02 EF is an 8% glass fiber reinforced UV-stabilized ABS/PA blend with enhanced dimensional stability, rigidity and high flowability.
Features: High dimensional stability; Excellent flow for high surface quality appearance; Enhanced softening temperature; Enhanced rigidity; UV-stabilized; Glass Fiber reinforced (8%)
Applications: Automotive parts; Motorcycle fairings; Truck cabin parts

Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North America

Filler/Reinforcement: Glass Fiber, 8% Filler by Weight

Additive: UV Stabilizer

Features: Good Dimensional Stability; Good Rigidity; Good Surface Finish; High Flow; UV Stabilized

Uses: Automotive Applications

Automotive Specifications: GM QK 002521 DU Color: 38308 Black

Form: Pellets

Information provided by INEOS Styrolution

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Bulk Density 0.550 - 0.650 g/cc
Density 1.12 g/ccISO 1183
Water Absorption 1.1 %Equilibrium, 50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.0050 - 0.0080 cm/cm
Melt Flow 40 g/10 min
@Load 10.0 kg,
Temperature 240 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Ball Indentation Hardness 14400 psiISO 2039-1
Tensile Strength, Yield 5970 psiISO 527-2
Elongation at Break 6.0 %Nominal; ISO 527-2
Elongation at Yield 3.0 %ISO 527-2
Tensile Modulus 450000 psiISO 527-1
Flexural Strength 12300 psiISO 178
Flexural Modulus 406000 psiISO 178
Izod Impact, Notched (ISO) 2.90 ft-lb/in²
@Temperature -30.0 °C
ISO 180/A
 5.70 ft-lb/in²
@Temperature 22.8 °C
ISO 180/A
Charpy Impact Unnotched 17.0 ft-lb/in²
@Temperature -30.0 °C
ISO 179/1eU
 24.0 ft-lb/in²
@Temperature 22.8 °C
ISO 179/1eU
Charpy Impact, Notched 2.90 ft-lb/in²
@Temperature -30.0 °C
ISO 179/1eA
 5.20 ft-lb/in²
@Temperature 22.8 °C
ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+15 ohm-cmIEC 62631-3-1
Surface Resistance 1.00e+14 ohmIEC 62631-3-1
Dielectric Constant 3.4
@Frequency 1e+6 Hz
IEC 62631-2-1
Dissipation Factor 0.018
@Frequency 1e+6 Hz
IEC 62631-2-1
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 33.0 µin/in-°FISO 11359-2
Deflection Temperature at 0.46 MPa (66 psi) 266 °FUnannealed; ISO 75-2/B
 340 °FAnnealed, 4H/80°C; ISO 75-2/B
Deflection Temperature at 1.8 MPa (264 psi) 176 °FUnannealed; ISO 75-2/A
 207 °FAnnealed, 4H/80°C; ISO 75-2/A
Vicat Softening Point 244 °FISO 306/B50
 392 °FISO 306/A50
Flammability, UL94 HB
@Thickness 1.52 mm
IEC 60695-11-10,-20
 
Processing PropertiesOriginal ValueComments
Melt Temperature 464 - 518 °F
Mold Temperature 140 - 176 °F
Drying Temperature 176 - 194 °F
Dry Time 4.00 - 8.00 hour

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSTYS774 / 311467

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.